GB/T 8163:2008 — Seamless steel tubes for liquid service

Chemical composition

wt% · log scale
0.010.11C0.17 – 0.23Cr0.25Cu0.25Mn0.35 – 0.65Ni0.3P0.035S0.035Si0.17 – 0.37
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥245 MPaTensile strength Rm410–530 MPaElongation A≥20 %Seamless tubes, Heat treated, <= 16 mmYield strength Rp0.2≥225 MPaTensile strength Rm410–530 MPaElongation A≥20 %Seamless tubes, Heat treated, > 16 mmYield strength Rp0.2≥235 MPaTensile strength Rm410–530 MPaElongation A≥20 %Seamless tubes, Heat treated, > 16 mm <= 30 mm

Chemical composition

ElementminmaxSimilarRemarks
C0.170.23
Cr0.25
Cu0.25
Mn0.350.65
Ni0.3
P0.035
S0.035
Si0.170.37

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
Seamless tubes, Heat treated, <= 16 mm≥245410–530≥20
Seamless tubes, Heat treated, > 16 mm≥225410–530≥20
Seamless tubes, Heat treated, > 16 mm <= 30 mm≥235410–530≥20