China · GB

20

GB/T 17396:2009 — Seamless hot-rolled steel tubes for hydraulic pillar service

Chemical composition

wt% · log scale
0.010.11C0.17 – 0.23Cr0.25Cu0.2Mn0.35 – 0.65Ni0.25P0.035S0.035Si0.17 – 0.37
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥235 MPaTensile strength Rm≥410 MPaElongation A≥20 %Seamless tubes, hot rolled, 16 < t <= 30 mmYield strength Rp0.2≥245 MPaTensile strength Rm≥410 MPaElongation A≥20 %Seamless tubes, hot rolled, t <= 16 mmYield strength Rp0.2≥225 MPaTensile strength Rm≥410 MPaElongation A≥20 %Seamless tubes, hot rolled, t > 30 mm

Chemical composition

ElementminmaxSimilarRemarks
C0.170.23
Cr0.25
Cu0.2
Mn0.350.65
Ni0.25
P0.035
S0.035
Si0.170.37

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
Seamless tubes, hot rolled, 16 < t <= 30 mm≥235≥410≥20
Seamless tubes, hot rolled, t <= 16 mm≥245≥410≥20
Seamless tubes, hot rolled, t > 30 mm≥225≥410≥20