GB 9948:2013 — Seamless steel tubes for petroleum cracking
Chemical composition
wt% · log scale- min – max range
- typical value
Mechanical properties
value range by conditionChemical composition
| Element | min | max | Similar | Remarks |
|---|---|---|---|---|
| C | 0.17 | 0.23 | ||
| Cr | 0.25 | |||
| Cu | 0.2 | |||
| Mn | 0.35 | 0.65 | ||
| Mo | 0.15 | |||
| Ni | 0.25 | |||
| P | 0.025 | |||
| S | 0.015 | |||
| Si | 0.17 | 0.37 | ||
| V | 0.08 |
Mechanical properties
| Heat treatment / condition | Yield strength | Tensile strength | Elongation | Reduction of area | Impact energy | Hardness |
|---|---|---|---|---|---|---|
| Seamless tubes | ≥245 | 410–550 | ≥22 Transverse;≥24 Longitudinal | ≥27 Transverse;≥40 Longitudinal |
Heat treatment
| Type | 3 | 4 |
|---|---|---|
| Heat-treatment process | Normalized | Normalizing temperature 880℃~940℃ |