China · GB

20

GB/T 3639:2009 — Seamless cold-drawn or cold-rolled steel tubes for precision applications

Chemical composition

wt% · log scale
0.010.11C0.17 – 0.23Cr0.25Cu0.25Mn0.35 – 0.65Ni0.3P0.035S0.035Si0.17 – 0.37
  • min – max range
  • typical value

Mechanical properties

value range by condition
Tensile strength Rm≥520 MPaElongation A≥8 %Seamless tubes +BKWYield strength Rp0.2≥375 MPaTensile strength Rm≥520 MPaElongation A≥12 %Seamless tubes +BKSTensile strength Rm≤550 MPaElongation A≤5 %Seamless tubes +BKYield strength Rp0.2≥255 MPaTensile strength Rm440–570 MPaElongation A≥21 %Seamless tubes +NBK

Chemical composition

ElementminmaxSimilarRemarks
C0.170.23
Cr0.25
Cu0.25
Mn0.350.65
Ni0.3
P0.035
S0.035
Si0.170.37

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
Seamless tubes +BKW≥520≥8
Seamless tubes +BKS≥375≥520≥12
Seamless tubes +BK≤550≤5
Seamless tubes +NBK≥255440–570≥21
Seamless tubes +GBK≥390≥21