Italy · UNI

C 55

UNI EN 10277-2 — Bright steel products - Technical delivery conditions - Part 2 : steels for general engineering purposes

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
bars +C, > 10 <= 16 mm≥520730–1080≥6
bars +C, > 16 <= 40 mm≥440690–1050≥7
bars +C, > 40 <= 63 mm≥390650–1030≥8
bars +C, >= 5 <= 10 mm≥590770–1100≥5
bars +SH, > 16 <= 100 mm490–630HB 181–269 HBW

Fatigue

Test conditions
ItemDetail
ProductSemi Finished products; Thickness: <= 16 mm; +QT
ExperimentReversed bending; T: 20°C
Specimen
Monotonic
PropertyValue
Yield strength (MPa)550.0
Tensile strength (MPa)800.0 950.0
Elongation (%)12.0
Reduction of area (%)30.0
Stress life
No.Cycles
11E7

Heat treatment

Type1
Heat-treatment curveHardness-Tempering