Italy · UNI

C 55

UNI 7065:1972 — UNI 7065

Chemical composition

ElementminmaxSimilarRemarks
C0.530.58
Mn0.40.65
P0.02
S0.02
Si0.35

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
steel strip, annealed≤550≥18 L0=80 mmHR ≤81 HRB;HB ≤152 HRB

Fatigue

Test conditions
ItemDetail
ProductSemi Finished products; Thickness: <= 16 mm; +QT
ExperimentReversed bending; T: 20°C
Specimen
Monotonic
PropertyValue
Yield strength (MPa)550.0
Tensile strength (MPa)800.0 950.0
Elongation (%)12.0
Reduction of area (%)30.0
Stress life
No.Cycles
11E7

Heat treatment

Type1
Heat-treatment curveHardness-Tempering