1.4563

BS EN 10088-3 — Stainless steels. Technical delivery conditions for semi-finished products,bars,rods,wire,sections and bright products of corrosion resisting steels for general purposes

Chemical composition

wt% · log scale
0.0010.010.1110100C0.02Cr26 – 28Cu0.7 – 1.5Mn2Mo3 – 4N0.11Ni30 – 32P0.03S0.01Si0.7
  • min – max range
  • typical value

Mechanical properties

value range by condition
Tensile strength Rm1100–1350 MPaWires +C1100, >= 0.05 mmTensile strength Rm600–800 MPaWires +C600, >= 0.05 mmTensile strength Rm700–900 MPaWires +C700, >= 0.05 mmTensile strength Rm800–1000 MPaWires +C800, >= 0.05 mm

High / low temperature

value vs. temperature
106129153176199100150200250300350400450500550°C
  • solution annealed +AT · Yield strength Rp0.2

Physical properties

vs. temperature
Elastic modulus GPa
158 – 195°C
Mean thermal expansion 10⁻⁶/K
15.8 – 17.3°C

Chemical composition

ElementminmaxSimilarRemarks
C0.02
Cr2628
Cu0.71.5
Mn2
Mo34
N0.11
Ni3032
P0.03
S0.01
Si0.7

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
Wires +C1100, >= 0.05 mm1100–1350
Wires +C600, >= 0.05 mm600–800
Wires +C700, >= 0.05 mm700–900
Wires +C800, >= 0.05 mm800–1000
Wires +C900, >= 0.05 mm900–1100
Wires +C1000, >= 0.05 mm1000–1250
Wires +C1200, >= 0.05 mm1200–1450
Wires +C1400, >= 0.05 mm1400–1700
Wires +C1600, >= 0.05 mm1600–1900
Wires +C1800, >= 0.05 mm1800–2100
Wires +C500, >= 0.05 mm500–700
Wires +AT, > 0.05 <= 0.1 mm≤1100≥20
Wires +AT, > 0.1 <= 0.2 mm≤1050≥20
Wires +AT, > 0.2 <= 0.5 mm≤1000≥30
Wires +AT, > 0.5 <= 1 mm≤950≥30
Wires +AT, > 1 <= 3 mm≤900≥30
Wires +AT, > 3 <= 5 mm≤850≥35
Wires +AT, > 5 <= 16 mm≤800≥35
rods, bars, wire, sections, bright products +AT, <= 160 mm≥220500–750≥35 After fracture; (trans.)≥100 KV (ISO-V) (trans.)HB ≤230
rods, bars, wire, sections, bright products +AT, > 160 <= 250 mm≥220500–750≥30 After fracture; (long.)≥60 KV (ISO-V) (trans.)HB ≤230

Physical properties

20.0

Elastic modulusMean thermal expansionThermal conductivitySpecific heatResistivityDensityPoisson's ratio
195.0012.00450.001.008.00

Typical physical values

DensityElastic modulusPoisson's ratioRemarks
7.61–8.10190.00–215.000.27–0.30Typical material properties for stainless steel. These values are not taken from the standard; they are indicative and must not be used for design.
7.86190.00–210.000.27–0.30Material properties for low-carbon, high-alloy steel. These values are not taken from the standard; they are indicative and must not be used for design.

High/low temperature

Yield strength Rp0.2 (MPa)
ConditionTemperature ℃Approx.
solution annealed +AT550115
solution annealed +AT500120
solution annealed +AT450125
solution annealed +AT400135
solution annealed +AT350145
solution annealed +AT300150
solution annealed +AT250155
solution annealed +AT200160
solution annealed +AT150175
solution annealed +AT100190

Similar grades

GradeRegionSystem
1.4563ItalyUNI
X 1 NiCrMoCu 31 27 4ItalyUNI
1.4563SpainUNE
X 1 NiCrMoCu 31 27 4SpainUNE
1.4563RomaniaSTAS
X 1 NiCrMoCu 31 27 4RomaniaSTAS
1.4563SwedenSS
X 1 NiCrMoCu 31 27 4SwedenSS
1.4563SwitzerlandSNV
X 1 NiCrMoCu 31 27 4SwitzerlandSNV
1.4563FinlandSFS
X 1 NiCrMoCu 31 27 4FinlandSFS
1.4563PolandPN
X 1 NiCrMoCu 31 27 4PolandPN
1.4563AustriaONORM
X 1 NiCrMoCu 31 27 4AustriaONORM
1.4563NorwayNS
X 1 NiCrMoCu 31 27 4NorwayNS
1.4563BelgiumNBN
X 1 NiCrMoCu 31 27 4BelgiumNBN
1.4563HungaryMSZ
X 1 NiCrMoCu 31 27 4HungaryMSZ
1.4563Czech RepublicCSN
X 1 NiCrMoCu 31 27 4Czech RepublicCSN
1.4563BulgariaBDS
X 1 NiCrMoCu 31 27 4BulgariaBDS
X 1 NiCrMoCu 31 27 4United KingdomB.S.
1.4563FranceAFNOR NF
X 1 NiCrMoCu 31 27 4FranceAFNOR NF
X 1 NiCrMoCu 31 27 4GermanyDIN
1.4563GermanyDIN