Czech Republic · CSN

X 2 CrNi 18 9

CSN EN 10250-4 — Open die steel forgings for general engineering purposes - Part 4 : stainless steels

Chemical composition

wt% · log scale
0.010.1110100C0.03Cr17.5 – 19.5Mn2N0.11Ni8 – 10P0.045S0.03Si1
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2175 MPaTensile strength Rm450 MPaImpact energy Kv/Ku60 JElongation A35 %Yield strength Rp0.2175 MPaTensile strength Rm450 MPaImpact energy Kv/Ku100 J

High / low temperature

value vs. temperature
72.292.4113133153100150200250300350400450500550°C
  • forgings Solution annealed · Yield strength Rp0.2

Physical properties

vs. temperature
Elastic modulus GPa
165 – 200°C
Mean thermal expansion 10⁻⁶/K
16.0 – 18.0°C

Creep properties

1.4444.287.0130173550560570580590600610620630640650660670680690700MPa
  • 10000.0h
  • 100000.0h

Temperature °C · time at rupture

Chemical composition

ElementminmaxSimilarRemarks
C0.03
Cr17.519.5
Mn2
N0.11
Ni810
P0.045
S0.03For products to be machined a controlled sulfur content of 0
Si1

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
die forgings, forgings, Solution annealed, <= 250 mm, forged bars175450 680.003560;100

Physical properties

20.0

Elastic modulusMean thermal expansionThermal conductivitySpecific heatResistivityDensityPoisson's ratio
200.0015.00500.000.737.90

Typical physical values

DensityElastic modulusPoisson's ratioRemarks
7.61–8.10190.00–215.000.27–0.30Typical material properties for stainless steel. These values are not taken from the standard; they are indicative and must not be used for design.
7.86190.00–210.000.27–0.30Material properties for low-carbon, high-alloy steel. These values are not taken from the standard; they are indicative and must not be used for design.

High/low temperature

Yield strength Rp0.2 (MPa)
ConditionTemperature ℃min
forgings Solution annealed55080
forgings Solution annealed50081
forgings Solution annealed45085
forgings Solution annealed40089
forgings Solution annealed35094
forgings Solution annealed300100
forgings Solution annealed250108
forgings Solution annealed200118
forgings Solution annealed150130
forgings Solution annealed100145

Creep

Temperature ℃Time hCRS
55010000.0h156.0
550100000.0h92.0
56010000.0h138.0
560100000.0h85.0
57010000.0h124.0
570100000.0h78.0
58010000.0h113.0
580100000.0h72.0
59010000.0h104.0
590100000.0h65.0
60010000.0h97.0
600100000.0h59.0
61010000.0h90.0
610100000.0h54.0
62010000.0h83.0
620100000.0h49.0
63010000.0h76.0
630100000.0h45.0
64010000.0h70.0
640100000.0h40.0
65010000.0h64.0
650100000.0h36.0
66010000.0h59.0
660100000.0h32.0
67010000.0h54.0
670100000.0h28.0
68010000.0h49.0
680100000.0h25.0
69010000.0h43.0
690100000.0h21.0
70010000.0h38.0
700100000.0h18.0

Similar grades

GradeRegionSystem
1.4307ItalyUNI
X 2 CrNi 18 9ItalyUNI
1.4307SpainUNE
X 2 CrNi 18 9SpainUNE
1.4307RomaniaSTAS
X 2 CrNi 18 9RomaniaSTAS
1.4307SwedenSS
X 2 CrNi 18 9SwedenSS
1.4307SwitzerlandSNV
X 2 CrNi 18 9SwitzerlandSNV
1.4307FinlandSFS
X 2 CrNi 18 9FinlandSFS
1.4307PolandPN
X 2 CrNi 18 9PolandPN
1.4307AustriaONORM
X 2 CrNi 18 9AustriaONORM
1.4307NorwayNS
X 2 CrNi 18 9NorwayNS
1.4307BelgiumNBN
X 2 CrNi 18 9BelgiumNBN
1.4307HungaryMSZ
X 2 CrNi 18 9HungaryMSZ
1.4307Czech RepublicCSN
1.4307BulgariaBDS
X 2 CrNi 18 9BulgariaBDS
1.4307United KingdomB.S.
X 2 CrNi 18 9United KingdomB.S.
1.4307FranceAFNOR NF
X 2 CrNi 18 9FranceAFNOR NF
X 2 CrNi 18 9GermanyDIN
1.4307GermanyDIN