Italy · UNI
X 2 CrNiMoN 17 13 3
UNI EN 10250-4 — Open die steel forgings for general engineering purposes - Part 4 : stainless steels
Chemical composition
wt% · log scale- min – max range
- typical value
Mechanical properties
value range by conditionHigh / low temperature
value vs. temperature- forgings Solution annealed · Yield strength Rp0.2
- forgings · Yield strength Rp0.2
- forgings · Tensile strength Rm
- forgings Solution annealed · Impact energy Kv/Ku
Physical properties
vs. temperatureChemical composition
| Element | min | max | Similar | Remarks |
|---|---|---|---|---|
| C | 0.03 | |||
| Cr | 16.5 | 18.5 | ||
| Mn | 2 | |||
| Mo | 2.5 | 3 | ||
| N | 0.12 | 0.22 | ||
| Ni | 11 | 14 | For fabrication where is necessary to minimize the delta ferrite content or with the aim of low permeability | |
| P | 0.045 | |||
| S | 0.015 | |||
| Si | 1 |
Mechanical properties
| Heat treatment / condition | Yield strength | Tensile strength | Elongation | Reduction of area | Impact energy | Hardness |
|---|---|---|---|---|---|---|
| die forgings, forgings, Solution annealed, <= 400 mm, forged bars | 280 | 580 800.00 | 30 | 60;100 | ||
| forgings, Solution annealed | ≥60 Charpy V Notch (-196°C);≥60 Charpy V Notch (-150°C) |
Physical properties
20.0
| Elastic modulus | Mean thermal expansion | Thermal conductivity | Specific heat | Resistivity | Density | Poisson's ratio |
|---|---|---|---|---|---|---|
| 200.00 | 15.00 | 500.00 | 0.75 | 8.00 |
Typical physical values
| Density | Elastic modulus | Poisson's ratio | Remarks |
|---|---|---|---|
| 7.61–8.10 | 190.00–215.00 | 0.27–0.30 | Typical material properties for stainless steel. These values are not taken from the standard; they are indicative and must not be used for design. |
| 7.86 | 190.00–210.00 | 0.27–0.30 | Material properties for low-carbon, high-alloy steel. These values are not taken from the standard; they are indicative and must not be used for design. |
High/low temperature
| Condition | Temperature ℃ | min | Approx. |
|---|---|---|---|
| forgings Solution annealed | 550 | 127 | |
| forgings Solution annealed | 500 | 129 | |
| forgings Solution annealed | 450 | 131 | |
| forgings Solution annealed | 400 | 135 | |
| forgings Solution annealed | 350 | 140 | |
| forgings Solution annealed | 300 | 145 | |
| forgings Solution annealed | 250 | 155 | |
| forgings Solution annealed | 200 | 167 | |
| forgings Solution annealed | 150 | 185 | |
| forgings Solution annealed | 100 | 211 | |
| forgings | -150 | 500 | |
| forgings | -196 | 600 |
| Condition | Temperature ℃ | Approx. |
|---|---|---|
| forgings | -150 | 1000 |
| forgings | -196 | 1150 |
| Condition | Temperature ℃ | min | Remarks |
|---|---|---|---|
| forgings Solution annealed | -150 | 60 | Charpy V Notch |
| forgings Solution annealed | -196 | 60 | Charpy V Notch |
| Condition | Temperature ℃ | Approx. |
|---|---|---|
| forgings | -150 | 30 |
| forgings | -196 | 30 |
Similar grades
| Grade | Region | System |
|---|---|---|
| X2CrNiMoN17-13-3 | International standard | ISO |
| 1.4429 | UNI | |
| 1.4429 | UNE | |
| 1.4429 | STAS | |
| X 2 CrNiMoN 17 13 3 | STAS | |
| 1.4429 | SS | |
| X 2 CrNiMoN 17 13 3 | SS | |
| 1.4429 | SNV | |
| X 2 CrNiMoN 17 13 3 | SNV | |
| 1.4429 | SFS | |
| X 2 CrNiMoN 17 13 3 | SFS | |
| 1.4429 | PN | |
| X 2 CrNiMoN 17 13 3 | PN | |
| 1.4429 | ONORM | |
| X 2 CrNiMoN 17 13 3 | ONORM | |
| 1.4429 | NS | |
| X 2 CrNiMoN 17 13 3 | NS | |
| 1.4429 | NBN | |
| X 2 CrNiMoN 17 13 3 | NBN | |
| 1.4429 | MSZ | |
| X 2 CrNiMoN 17 13 3 | MSZ | |
| 1.4429 | Czech Republic | CSN |
| X 2 CrNiMoN 17 13 3 | Czech Republic | CSN |
| 1.4429 | Bulgaria | BDS |
| X 2 CrNiMoN 17 13 3 | Bulgaria | BDS |
| 1.4429 | B.S. | |
| X 2 CrNiMoN 17 13 3 | B.S. | |
| 1.4429 | AFNOR NF | |
| X 2 CrNiMoN 17 13 3 | UNE | |
| X 2 CrNiMoN 17 13 3 | AFNOR NF | |
| X 2 CrNiMoN 17 13 3 | DIN | |
| 1.4429 | DIN |