Italy · UNI

X 2 CrNiMoN 17 13 3

UNI EN 10088-3 — Stainless steels. Technical delivery conditions for semi-finished products, bars, rods and sections for general purposes.

Chemical composition

wt% · log scale
0.0010.010.1110100C0.03Cr16.5 – 18.5Mn2Mo2.5 – 3N0.12 – 0.22Ni11 – 14P0.045S0.015Si1
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥280 MPaTensile strength Rm580–800 MPaImpact energy Kv/Ku≥100 JElongation A≥40 %rods, bars, wire, sections, bright products +AT, <= 160 mmYield strength Rp0.2≥280 MPaTensile strength Rm580–800 MPaImpact energy Kv/Ku≥60 JElongation A≥30 %rods, bars, wire, sections, bright products +AT, > 160 <= 250 mm

High / low temperature

value vs. temperature
127151176200224100150200250300350400450500550°C
  • solution annealed +AT · Yield strength Rp0.2

Physical properties

vs. temperature
Elastic modulus GPa
165 – 200°C
Mean thermal expansion 10⁻⁶/K
16.0 – 18.0°C

Chemical composition

ElementminmaxSimilarRemarks
C0.03
Cr16.518.5
Mn2
Mo2.53
N0.120.22
Ni1114For special reasons (minimize the delta ferrite content) the maximum content of Ni= 1
P0.045
S0.015
Si1

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
rods, bars, wire, sections, bright products +AT, <= 160 mm≥280580–800≥40 After fracture; (trans.)≥100 KV (ISO-V) (trans.)
rods, bars, wire, sections, bright products +AT, > 160 <= 250 mm≥280580–800≥30 After fracture; (long.)≥60 KV (ISO-V) (trans.)

Physical properties

20.0

Elastic modulusMean thermal expansionThermal conductivitySpecific heatResistivityDensityPoisson's ratio
200.0015.00500.000.758.00

Typical physical values

DensityElastic modulusPoisson's ratioRemarks
7.61–8.10190.00–215.000.27–0.30Typical material properties for stainless steel. These values are not taken from the standard; they are indicative and must not be used for design.
7.86190.00–210.000.27–0.30Material properties for low-carbon, high-alloy steel. These values are not taken from the standard; they are indicative and must not be used for design.

High/low temperature

Yield strength Rp0.2 (MPa)
ConditionTemperature ℃Approx.
solution annealed +AT550136
solution annealed +AT500138
solution annealed +AT450140
solution annealed +AT400145
solution annealed +AT350150
solution annealed +AT300155
solution annealed +AT250165
solution annealed +AT200175
solution annealed +AT150195
solution annealed +AT100215

Similar grades

GradeRegionSystem
X2CrNiMoN17-13-3International standardISO
1.4429ItalyUNI
1.4429SpainUNE
1.4429RomaniaSTAS
X 2 CrNiMoN 17 13 3RomaniaSTAS
1.4429SwedenSS
X 2 CrNiMoN 17 13 3SwedenSS
1.4429SwitzerlandSNV
X 2 CrNiMoN 17 13 3SwitzerlandSNV
1.4429FinlandSFS
X 2 CrNiMoN 17 13 3FinlandSFS
1.4429PolandPN
X 2 CrNiMoN 17 13 3PolandPN
1.4429AustriaONORM
X 2 CrNiMoN 17 13 3AustriaONORM
1.4429NorwayNS
X 2 CrNiMoN 17 13 3NorwayNS
1.4429BelgiumNBN
X 2 CrNiMoN 17 13 3BelgiumNBN
1.4429HungaryMSZ
X 2 CrNiMoN 17 13 3HungaryMSZ
1.4429Czech RepublicCSN
X 2 CrNiMoN 17 13 3Czech RepublicCSN
1.4429BulgariaBDS
X 2 CrNiMoN 17 13 3BulgariaBDS
1.4429United KingdomB.S.
X 2 CrNiMoN 17 13 3United KingdomB.S.
1.4429FranceAFNOR NF
X 2 CrNiMoN 17 13 3SpainUNE
X 2 CrNiMoN 17 13 3FranceAFNOR NF
X 2 CrNiMoN 17 13 3GermanyDIN
1.4429GermanyDIN