China · GB

15

GB/T 13793:2008 — Steel pipes with a longitudinal electric (resistance) weld

Chemical composition

wt% · log scale
0.010.11C0.12 – 0.18Cr0.25Cu0.25Mn0.35 – 0.65Ni0.3P0.035S0.035Si0.17 – 0.37
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥215 MPaYield strength Rp0.2≥225 MPaTensile strength Rm≥355 MPaTensile strength Rm≥400 MPaTensile strength Rm≥355 MPaElongation A≥20 %Elongation A≥11 %

Chemical composition

ElementminmaxSimilarRemarks
C0.120.18
Cr0.25
Cu0.25
Mn0.350.65
Ni0.3
P0.035
S0.035
Si0.170.37

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
steel tubes, welded≥215;≥225≥355;≥400≥20;≥11