Chemical composition
| Element | min | max | Similar | Remarks |
|---|---|---|---|---|
| Al | 0.02 | If nitrogen is additionally fixed by niobium | If nitrogen is additionally fixed by niobium | |
| C | 0.18 | |||
| Cr | 0.3 | |||
| Cr+Cu+Mo | 0.45 | |||
| Cu | 0.2 | |||
| Mn | 0.6 | 1.4 | ||
| Mo | 0.08 | |||
| N | 0.02 | |||
| Nb | 0.03 | |||
| Nb+Ti+V | 0.05 | |||
| Ni | 0.3 | |||
| P | 0.035 | |||
| S | 0.03 | |||
| Si | 0.4 |
Mechanical properties
| Heat treatment / condition | Yield strength | Tensile strength | Elongation | Reduction of area | Impact energy | Hardness |
|---|---|---|---|---|---|---|
| steel tubes, normalized, t <=, 20 mm | ≥285 Upper Yield Stress | 390–510 | ≥24 Parallel to the tube axis | ≥39 Charpy V Notch -20°C |
Physical properties
-100.0
| Elastic modulus | Mean thermal expansion | Thermal conductivity | Specific heat | Resistivity | Density | Poisson's ratio |
|---|---|---|---|---|---|---|
| 217.00 | 10.80 | 52.60 | 371.00 | 0.13 |
Typical physical values
| Density | Elastic modulus | Poisson's ratio | Remarks |
|---|---|---|---|
| 7.86 | 203.00 | 0.27–0.30 | 低碳,低合金钢的典型性能数值。此值不来源于标准,它是指示性指标,不能被用于设计用途。 |
High/low temperature
| Condition | Temperature ℃ | min | Remarks |
|---|---|---|---|
| steel tubes normalized t <= 20 mm | -20 | 39 | Charpy V Notch |
Similar grades
| Grade | Region | System |
|---|---|---|
| StE 285 | SEW | |
| 1.0486 | DIN |