Germany · DIN

StE 285

DIN 17102:1983 — DIN 17102

Chemical composition

ElementminmaxSimilarRemarks
Al0.02If nitrogen is additionally fixed by niobiumIf nitrogen is additionally fixed by niobium
C0.18
Cr0.3
Cr+Cu+Mo0.45
Cu0.2
Mn0.61.4
Mo0.08
Nb0.03
Nb+Ti+V0.05
Ni0.3
P0.035
S0.03
Si0.4

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
bars, sections 100 < t ≤ 125mm, hot rolled, flats235360 480.0024
bars, sections 125 < t ≤ 150mm, hot rolled, flats225350 460.0024
bars, sections 35 < t ≤ 50mm, hot rolled, flats276390 510.0024
bars, sections 50 < t ≤ 70mm, hot rolled, flats265390 510.0024
bars, sections 70 < t ≤ 85mm, hot rolled, flats255380 500.0024
bars, sections 85 < t ≤ 100mm, hot rolled, flats245370 490.0024
bars, sections t ≤ 35mm, hot rolled, flats285390 510.0024

Physical properties

-100.0

Elastic modulusMean thermal expansionThermal conductivitySpecific heatResistivityDensityPoisson's ratio
217.0010.8052.60371.000.13

Typical physical values

DensityElastic modulusPoisson's ratioRemarks
7.86203.000.27–0.30低碳,低合金钢的典型性能数值。此值不来源于标准,它是指示性指标,不能被用于设计用途。

Similar grades

GradeRegionSystem
StE 285GermanySEW
1.0486GermanyDIN