Poland · PN

1.4539

PN EN 10088-3

Chemical composition

wt% · log scale
0.0010.010.1110100C0.02Cr19 – 21Cu1.2 – 2Mn2Mo4 – 5N0.15Ni24 – 26P0.03S0.01Si0.7
  • min – max range
  • typical value

Mechanical properties

value range by condition
Tensile strength Rm1100–1350 MPaWires +C1100, >= 0.05 mmTensile strength Rm600–800 MPaWires +C600, >= 0.05 mmTensile strength Rm700–900 MPaWires +C700, >= 0.05 mmTensile strength Rm800–1000 MPaWires +C800, >= 0.05 mm

High / low temperature

value vs. temperature
93.0124155186217100150200250300350400450500550°C
  • solution annealed +AT · Yield strength Rp0.2

Physical properties

vs. temperature
Elastic modulus GPa
158 – 195°C
Mean thermal expansion 10⁻⁶/K
15.8 – 17.3°C

Chemical composition

ElementminmaxSimilarRemarks
C0.02
Cr1921
Cu1.22
Mn2
Mo45
N0.15
Ni2426
P0.03
S0.01
Si0.7

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
Wires +C1100, >= 0.05 mm1100–1350
Wires +C600, >= 0.05 mm600–800
Wires +C700, >= 0.05 mm700–900
Wires +C800, >= 0.05 mm800–1000
Wires +C900, >= 0.05 mm900–1100
Wires +C1000, >= 0.05 mm1000–1250
Wires +C1200, >= 0.05 mm1200–1450
Wires +C1400, >= 0.05 mm1400–1700
Wires +C1600, >= 0.05 mm1600–1900
Wires +C1800, >= 0.05 mm1800–2100
Wires +C500, >= 0.05 mm500–700
Wires +AT, > 0.05 <= 0.1 mm≤1100≥20
Wires +AT, > 0.1 <= 0.2 mm≤1050≥20
Wires +AT, > 0.2 <= 0.5 mm≤1000≥30
Wires +AT, > 0.5 <= 1 mm≤950≥30
Wires +AT, > 1 <= 3 mm≤900≥30
Wires +AT, > 3 <= 5 mm≤850≥35
Wires +AT, > 5 <= 16 mm≤800≥35
rods, bars, wire, sections, bright products +AT, <= 160 mm≥230530–730≥35 After fracture; (trans.)≥100 KV (ISO-V) (trans.)HB ≤230
rods, bars, wire, sections, bright products +AT, > 160 <= 250 mm≥200530–730≥30 After fracture; (long.)≥60 KV (ISO-V) (trans.)
bars +AT, <= 16, mm≥400600–930≥20 (Longitudinal)
bars +AT, > 16 <= 63 mm≥230530–880≥25 (Longitudinal)≥100 (Longitudinal)
bars +AT, > 160 <= 250 mm≥230530–730≥30 (Transverse)≥60 (Transverse)
bars +AT, > 63 <= 160 mm≥230530–730≥35 (Longitudinal)≥100 (Longitudinal)

Physical properties

20.0

Elastic modulusMean thermal expansionThermal conductivitySpecific heatResistivityDensityPoisson's ratio
195.00;180.00;185.0012.00450.001.008.00

Typical physical values

DensityElastic modulusPoisson's ratioRemarks
7.61–8.10190.00–215.000.27–0.30Typical material properties for stainless steel. These values are not taken from the standard; they are indicative and must not be used for design.
7.86190.00–210.000.27–0.30Material properties for low-carbon, high-alloy steel. These values are not taken from the standard; they are indicative and must not be used for design.

High/low temperature

Yield strength Rp0.2 (MPa)
ConditionTemperature ℃Approx.
solution annealed +AT550105
solution annealed +AT500110
solution annealed +AT450115
solution annealed +AT400125
solution annealed +AT350135
solution annealed +AT300145
solution annealed +AT250160
solution annealed +AT200175
solution annealed +AT150190
solution annealed +AT100205

Similar grades

GradeRegionSystem
1.4539ItalyUNI
X 1 NiCrMoCu 25 20 5ItalyUNI
1.4539SpainUNE
X 1 NiCrMoCu 25 20 5SpainUNE
1.4539RomaniaSTAS
X 1 NiCrMoCu 25 20 5RomaniaSTAS
1.4539SwedenSS
X 1 NiCrMoCu 25 20 5SwedenSS
1.4539SwitzerlandSNV
X 1 NiCrMoCu 25 20 5SwitzerlandSNV
1.4539FinlandSFS
X 1 NiCrMoCu 25 20 5FinlandSFS
X 1 NiCrMoCu 25 20 5PolandPN
1.4539AustriaONORM
X 1 NiCrMoCu 25 20 5AustriaONORM
1.4539NorwayNS
X 1 NiCrMoCu 25 20 5NorwayNS
1.4539BelgiumNBN
X 1 NiCrMoCu 25 20 5BelgiumNBN
1.4539HungaryMSZ
X 1 NiCrMoCu 25 20 5HungaryMSZ
1.4539Czech RepublicCSN
X 1 NiCrMoCu 25 20 5Czech RepublicCSN
1.4539BulgariaBDS
X 1 NiCrMoCu 25 20 5BulgariaBDS
1.4539United KingdomB.S.
X 1 NiCrMoCu 25 20 5United KingdomB.S.
1.4539FranceAFNOR NF
X1NiCrMoCu25-20-5International standardISO
X 1 NiCrMoCu 25 20 5FranceAFNOR NF
X 1 NiCrMoCu 25 20 5GermanyDIN
1.4539GermanyDIN