Czech Republic · CSN

25 CrMo 4

CSN EN 2206

Chemical composition

wt% · log scale
0.0010.010.1110C0.22 – 0.29Cr0.9 – 1.2Mn0.5 – 0.8Mo0.15 – 0.25Ni0.3P0.02S0.015Si0.1 – 0.35
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥480 MPaTensile strength Rm650–850 MPaImpact energy Kv/Ku≥35 JElongation A≥11 %HardnessHBYield strength Rp0.2≥480 MPaTensile strength Rm650–850 MPaImpact energy Kv/Ku≥70 JElongation A≥15 %HardnessHBbars, hardened tempered, <= 150 mmHardnessHBbars +A, <= 150 mm

Physical properties

vs. temperature
Elastic modulus GPa
164 – 217°C
Mean thermal expansion 10⁻⁶/K
10.5 – 14.4°C
Thermal conductivity W/(m·K)
34.4 – 42.8°C
Specific heat J/(kg·K)
371 – 778°C
Resistivity Ω·mm²/m
0.250 – 0.810°C

Creep properties

-6.12103212320429420430440450460470480490500510520530540550MPa
  • 10000.0h
  • 100000.0h

Temperature °C · time at rupture

Chemical composition

ElementminmaxSimilarRemarks
C0.220.29
Cr0.91.2
Mn0.50.8
Mo0.150.25
Ni0.3
P0.02
S0.015
Si0.10.35

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
bars, hardened tempered, <= 150 mm≥480650–850≥11;≥15≥35 KV (20°C) long.;≥70 KV (20°C) long.HB 197–255
bars +A, <= 150 mmHB ≤212

Physical properties

-100.0

Elastic modulusMean thermal expansionThermal conductivitySpecific heatResistivityDensityPoisson's ratio
217.0010.50371.00

Typical physical values

DensityElastic modulusPoisson's ratioRemarks
7.86203.000.27–0.30Typical properties for low-carbon, low-alloy steel. These values are not taken from the standard; they are indicative and must not be used for design.

Fatigue

Test conditions
ItemDetail
ProductSemi Finished products; Thickness: <= 16 mm; +QT
ExperimentReversed bending; T: 20°C
Specimen
Monotonic
PropertyValue
Yield strength (MPa)700.0
Tensile strength (MPa)900.0 1100.0
Elongation (%)12.0
Reduction of area (%)50.0
Stress life
No.Cycles
11E7

Creep

Temperature ℃Time hRp1CRS
42010000.0h274.0387.0
420100000.0h221.0308.0
43010000.0h258.0364.0
430100000.0h203.0281.0
44010000.0h242.0338.0
440100000.0h186.0253.0
45010000.0h226.0311.0
450100000.0h171.0226.0
46010000.0h210.0283.0
460100000.0h155.0200.0
47010000.0h195.0255.0
470100000.0h141.0178.0
48010000.0h180.0226.0
480100000.0h127.0157.0
49010000.0h163.0200.0
490100000.0h112.0136.0
50010000.0h147.0176.0
500100000.0h98.0118.0
51010000.0h130.0153.0
510100000.0h83.0100.0
52010000.0h115.0133.0
520100000.0h69.082.0
53010000.0h98.0114.0
530100000.0h54.066.0
54010000.0h81.095.0
540100000.0h39.051.0
55010000.0h64.079.0
550100000.0h25.036.0

Heat treatment

Type1
Heat-treatment curveHardness-Tempering
Heat-treatment curveCCT modified
Heat-treatment curveCCT
Heat-treatment curveTTT
Heat-treatment curveHardenability

Similar grades

GradeRegionSystem
1.7218ItalyUNI
1.7218SpainUNE
1.7218RomaniaSTAS
25 CrMo 4RomaniaSTAS
1.7218SwedenSS
25 CrMo 4SwedenSS
1.7218SwitzerlandSNV
25 CrMo 4SwitzerlandSNV
1.7218FinlandSFS
25 CrMo 4FinlandSFS
1.7218PolandPN
25 CrMo 4PolandPN
1.7218AustriaONORM
25 CrMo 4AustriaONORM
1.7218NorwayNS
1.7218BelgiumNBN
1.7218HungaryMSZ
25 CrMo 4HungaryMSZ
1.7218Czech RepublicCSN
1.7218BulgariaBDS
25 CrMo 4BulgariaBDS
1.7218United KingdomB.S.
1.7218FranceAFNOR NF
25 CrMo 4NorwayNS
25 CrMo 4BelgiumNBN
25 CrMo 4SpainUNE
25 CrMo 4ItalyUNI
25 CrMo 4FranceAFNOR NF
25 CrMo 4GermanyDIN
1.7218GermanyDIN
25 CrMo 4United KingdomB.S.