Czech Republic · CSN

25 CrMo 4

CSN EN 10250-3 — Open steel die forgings for general engineering purposes. Alloy special steels

Chemical composition

wt% · log scale
0.010.1110C0.22 – 0.29Cr0.9 – 1.2Mn0.6 – 0.9Mo0.15 – 0.3P0.035S0.035Si0.4
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2450 MPaTensile strength Rm700 MPaImpact energy Kv/Ku50 JElongation A15 %die forgings, forgings, quenched and tempered, <= 70 mm, forged barsYield strength Rp0.2380 MPaTensile strength Rm600 MPaImpact energy Kv/Ku22 JElongation A14 %Yield strength Rp0.2380 MPaTensile strength Rm600 MPaImpact energy Kv/Ku38 JElongation A18 %die forgings, forgings, quenched and tempered, > 160 <= 330 mm, forged barsYield strength Rp0.2400 MPaTensile strength Rm650 MPaImpact energy Kv/Ku27 JElongation A13 %Yield strength Rp0.2400 MPaTensile strength Rm650 MPaImpact energy Kv/Ku45 JElongation A17 %die forgings, forgings, quenched and tempered, > 70 <= 160 mm, forged bars

Physical properties

vs. temperature
Elastic modulus GPa
164 – 217°C
Mean thermal expansion 10⁻⁶/K
10.5 – 14.4°C
Thermal conductivity W/(m·K)
34.4 – 42.8°C
Specific heat J/(kg·K)
371 – 778°C
Resistivity Ω·mm²/m
0.250 – 0.810°C

Creep properties

-6.12103212320429420430440450460470480490500510520530540550MPa
  • 10000.0h
  • 100000.0h

Temperature °C · time at rupture

Chemical composition

ElementminmaxSimilarRemarks
C0.220.29
Cr0.91.2
Mn0.60.9
Mo0.150.3
P0.035
S0.035
Si0.4

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
die forgings, forgings, quenched and tempered, <= 70 mm, forged bars4507001550
die forgings, forgings, quenched and tempered, > 160 <= 330 mm, forged bars38060014;1822;38
die forgings, forgings, quenched and tempered, > 70 <= 160 mm, forged bars40065013;1727;45

Physical properties

-100.0

Elastic modulusMean thermal expansionThermal conductivitySpecific heatResistivityDensityPoisson's ratio
217.0010.50371.00

Typical physical values

DensityElastic modulusPoisson's ratioRemarks
7.86203.000.27–0.30Typical properties for low-carbon, low-alloy steel. These values are not taken from the standard; they are indicative and must not be used for design.

Fatigue

Test conditions
ItemDetail
ProductSemi Finished products; Thickness: <= 16 mm; +QT
ExperimentReversed bending; T: 20°C
Specimen
Monotonic
PropertyValue
Yield strength (MPa)700.0
Tensile strength (MPa)900.0 1100.0
Elongation (%)12.0
Reduction of area (%)50.0
Stress life
No.Cycles
11E7

Creep

Temperature ℃Time hRp1CRS
42010000.0h274.0387.0
420100000.0h221.0308.0
43010000.0h258.0364.0
430100000.0h203.0281.0
44010000.0h242.0338.0
440100000.0h186.0253.0
45010000.0h226.0311.0
450100000.0h171.0226.0
46010000.0h210.0283.0
460100000.0h155.0200.0
47010000.0h195.0255.0
470100000.0h141.0178.0
48010000.0h180.0226.0
480100000.0h127.0157.0
49010000.0h163.0200.0
490100000.0h112.0136.0
50010000.0h147.0176.0
500100000.0h98.0118.0
51010000.0h130.0153.0
510100000.0h83.0100.0
52010000.0h115.0133.0
520100000.0h69.082.0
53010000.0h98.0114.0
530100000.0h54.066.0
54010000.0h81.095.0
540100000.0h39.051.0
55010000.0h64.079.0
550100000.0h25.036.0

Heat treatment

Type1
Heat-treatment curveHardness-Tempering
Heat-treatment curveCCT modified
Heat-treatment curveCCT
Heat-treatment curveTTT
Heat-treatment curveHardenability

Similar grades

GradeRegionSystem
1.7218ItalyUNI
1.7218SpainUNE
1.7218RomaniaSTAS
25 CrMo 4RomaniaSTAS
1.7218SwedenSS
25 CrMo 4SwedenSS
1.7218SwitzerlandSNV
25 CrMo 4SwitzerlandSNV
1.7218FinlandSFS
25 CrMo 4FinlandSFS
1.7218PolandPN
25 CrMo 4PolandPN
1.7218AustriaONORM
25 CrMo 4AustriaONORM
1.7218NorwayNS
1.7218BelgiumNBN
1.7218HungaryMSZ
25 CrMo 4HungaryMSZ
1.7218Czech RepublicCSN
1.7218BulgariaBDS
25 CrMo 4BulgariaBDS
1.7218United KingdomB.S.
1.7218FranceAFNOR NF
25 CrMo 4NorwayNS
25 CrMo 4BelgiumNBN
25 CrMo 4SpainUNE
25 CrMo 4ItalyUNI
25 CrMo 4FranceAFNOR NF
25 CrMo 4GermanyDIN
1.7218GermanyDIN
25 CrMo 4United KingdomB.S.