United States · ASTM
B435 R30556
ASTM B435:2011 — Standard Specification for UNS N06002, UNS N06230, UNS N12160, and UNS R30556 Plate, Sheet, and Strip
Chemical composition
wt% · log scale- min – max range
- typical value
Mechanical properties
value range by conditionChemical composition
| Element | min | max | Similar | Remarks |
|---|---|---|---|---|
| Al | 0.1 | 0.5 | ||
| B | 0.02 | |||
| C | 0.05 | 0.15 | ||
| Cb | 0.3 | |||
| Co | 16 | 21 | ||
| Cr | 21 | 23 | ||
| Fe | Bal | |||
| La | 0.005 | 0.1 | ||
| Mn | 0.5 | 2 | ||
| Mo | 2.5 | 4 | ||
| N | 0.1 | 0.3 | ||
| Ni | 19 | 22.5 | ||
| P | 0.04 | |||
| S | 0.015 | |||
| Si | 0.2 | 0.8 | ||
| Ta | 0.3 | 1.25 | ||
| W | 2 | 3.5 | ||
| Zr | 0.001 | 0.1 |
Mechanical properties
| Heat treatment / condition | Yield strength | Tensile strength | Elongation | Reduction of area | Impact energy | Hardness |
|---|---|---|---|---|---|---|
| heavy plate, steel strip, Heat treated, t >= 4.76 mm +P; t < 4.76 mm +S +P - plates; +S - sheets, strips, sheet | 310.00 | 690.00 | 40.00 |