Czech Republic · CSN

EN AW-2014A

CSN EN 754-2 — Aluminium and aluminium alloys. Cold drawn rod/bar and tube. Mechanical properties

Chemical composition

wt% · log scale
0.010.1110Cr0.1Cu3.9 – 5Fe0.5Mg0.2 – 0.8Mn0.4 – 1.2Ni0.1Others each0.05Si0.5 – 0.9Ti0.15Ti+Zr0.2Total Others0.15Zn0.25
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≤125 MPaTensile strength Rm≤240 MPaElongation A≥12 %Drawn bars/rods, Annealed +O, <= 80 mm +T - thickness; +A - areaYield strength Rp0.2≥380 MPaTensile strength Rm≥450 MPaElongation A≥8 %Drawn bars/rods, Solution heat treated and artificially aged , <= 80 mmYield strength Rp0.2≥220 MPaTensile strength Rm≥380 MPaElongation A≥8 %Drawn bars/rods, Solution heat treated and naturally aged , <= 80 mm +T - thickness; +A - areaYield strength Rp0.2≥220 MPaTensile strength Rm≥380 MPaElongation A≥10 %Drawn bars/rods, Solution heat treated and naturally aged +T451, <= 80 mm +T - thickness; +A - area

Chemical composition

ElementminmaxSimilarRemarks
Al​​Bal​​
Cr0.1
Cu3.95
Fe0.5
Mg0.20.8
Mn0.41.2
Ni0.1
Others each0.05Includes listed elements for which no specific limit is shown.
Si0.50.9
Ti0.15
Ti+Zr0.2
Total Others0.15The sum of those "Others" metallic elements 0.010% or more each
Zn0.25

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
Drawn bars/rods, Annealed +O, <= 80 mm +T - thickness; +A - area≤125≤240≥12
Drawn bars/rods, Solution heat treated and artificially aged , <= 80 mm≥380≥450≥8
Drawn bars/rods, Solution heat treated and naturally aged , <= 80 mm +T - thickness; +A - area≥220≥380≥8
Drawn bars/rods, Solution heat treated and naturally aged +T451, <= 80 mm +T - thickness; +A - area≥220≥380≥10
Drawn bars/rods, Solution heat treated, cold worked and naturally aged , <= 80 mm +T - thickness; +A - area≤290≤380≤8
Drawn bars/rods, Solution heat treated, cold worked and naturally aged +T351, <= 80 mm +T - thickness; +A - area≤290≤380≤6
Drawn bars/rods, Strain-hardened only +H111, <= 80 mm +T - thickness; +A - area≤125≤240≥12
Drawn bars/rods, solution heat treated artificially aged, <= 80 mm≥380≥450≥8
Drawn tubes, Annealed +O, <= 20 mm +T - thickness; +A - area≤125≤240≥12
Drawn tubes, Solution heat treated and artificially aged +T6510, <= 20 mm≥380≥450≥8
Drawn tubes, Solution heat treated and artificially aged +T6511, <= 20 mm≥380≥450≥8
Drawn tubes, Solution heat treated and naturally aged , <= 20 mm +T - thickness; +A - area≥240≥380≥12
Drawn tubes, Solution heat treated and naturally aged +T4510, <= 20 mm +T - thickness; +A - area≥240≥380≥10
Drawn tubes, Solution heat treated and naturally aged +T4511, <= 20 mm +T - thickness; +A - area≥240≥380≥10
Drawn tubes, Solution heat treated, cold worked and naturally aged , <= 20 mm +T - thickness; +A - area≤290≤380≤8
Drawn tubes, Solution heat treated, cold worked and naturally aged +T3510, <= 20 mm +T - thickness; +A - area≤290≤380≤6
Drawn tubes, Solution heat treated, cold worked and naturally aged +T3511, <= 20 mm +T - thickness; +A - area≤290≤380≤6
Drawn tubes, Strain-hardened only +H111, <= 20 mm +T - thickness; +A - area≤125≤240≥12
Drawn tubes, solution heat treated artificially aged, <= 20 mm≥380≥450≥8