Hungary · MSZ

CB754S

MSZ EN 1982

Chemical composition

wt% · log scale
0.010.1110100Al0.1 – 0.8Cu58 – 62Fe0.7Mn0.5Ni1P0.02Pb0.5 – 2.4Si0.05Sn1
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥120 MPaTensile strength Rm≥280 MPaElongation A≥10 %HardnessHBCentrifugal castings +GZYield strength Rp0.2≥120 MPaTensile strength Rm≥280 MPaElongation A≥10 %HardnessHBPermanent mould castings +GMYield strength Rp0.2≥250 MPaTensile strength Rm≥350 MPaElongation A≥4 %HardnessHBPressure die castings +GPYield strength Rp0.2≥80 MPaTensile strength Rm≥220 MPaElongation A≥15 %HardnessHBSand castings +GS

Chemical composition

ElementminmaxSimilarRemarks
Al0.10.8
Cu5862Analysis value for Cu may contain NiAnalysis value for Cu may contain Ni
Fe0.7
Mn0.5
Ni1
P0.02
Pb0.52.4
Si0.05
Sn1
Zn​​Bal​​​​Bal​​

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
Centrifugal castings +GZ≥120≥280≥10HB ≥70
Permanent mould castings +GM≥120≥280≥10HB ≥70
Pressure die castings +GP≥250≥350≥4HB ≥110
Sand castings +GS≥80≥220≥15HB ≥65