Inconel 706

-- — -

Chemical composition

ElementminmaxSimilarRemarks
Al0.4
B0.006
C0.06
Co1
Cr14.517.5
Cu0.3
Fe​​Bal​​​​Bal​​
Mn0.35
Nb2.53.3Nb+TaNb+Ta
Ni3944plus Coplus Co
P0.02
S0.015
Si0.35
Ti1.52

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
Cold rolled sheets, Solution treated, t = 1.02 mm≥383≥757≥47
Cold rolled sheets, solution treated-precipitation hardened, t = 1.02≥1112≥1334≥24
Cold rolled sheets, solution treated-precipitation hardened, t = 1.57 mm≥1096≥1317≥20
Cold rolled sheets, solution treated hardened, t = 1.02 mm≥1024≥1282≥22
Cold rolled sheets, solution treated hardened, t = 1.57 mm≥1058≥1303≥18
solution treated-precipitation hardened, d = 14.3 mm≥1089≥1331≥21
solution treated hardened, d = 14.3 mm≥993≥1282≥19
solution treated hardened, d = 203 mm≥1007≥1303≥18
solution treated-precipitation hardened, t = 31.8 mm≥1114≥1334≥20
steel bars, solution treated-precipitation hardened, d = 14.3 mm≥1089≥1331≥21
steel bars, solution treated hardened, d = 14.3 mm≥1072≥1324≥16
forged , Solution treated≥288≥745≥50
forged , solution treated-precipitation hardened≥1085≥1262≥22
forged , solution treated hardened≥979≥1245≥17

Physical properties

-196.0

Elastic modulusMean thermal expansionThermal conductivitySpecific heatResistivityDensityPoisson's ratio
218.007.900.88