United States · AMS

355

SAE AMS 4280J:2008 — SAE AMS 4280J

Chemical composition

wt% · log scale
0.010.1110Cr0.25Cu1 – 1.5Fe0.6Mg0.4 – 0.6Mn0.5Si4.5 – 5.5Ti0.25Total Each0.05Total Others0.15Zn0.35
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥138 MPaTensile strength Rm≥176 MPaHardnessHBYield strength Rp0.2≥186 MPaTensile strength Rm≥234 MPaElongation A≥1 %HardnessHB

Physical properties

vs. temperature
Mean thermal expansion 10⁻⁶/K
21.3 – 24.2°C

Chemical composition

ElementminmaxSimilarRemarks
Al​​Bal​​​​Bal​​
Cr0.25
Cu11.5
Fe0.6
Mg0.40.6
Mn0.5
Si4.55.5
Ti0.25
Total Each0.05
Total Others0.15
Zn0.35

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
Permanent mould castings, Solution heat treated and artificially overaged +T71≥138;≥186≥176;≥234≥1 Lo= 50.8 mm;HB 70–95 HB/10/500 od Hardness min.=75-100 HB/10/1000

Physical properties

20.0

Elastic modulusMean thermal expansionThermal conductivitySpecific heatResistivityDensityPoisson's ratio
21.47

Typical physical values

DensityElastic modulusPoisson's ratioRemarks
2.60–2.9069.00–79.000.33典型性能值: 铝合金。该数值并非来自发行标准,它仅是指标性的,不能用于设计用途。