Global · Enterprise standard
Hastelloy C-22HS
-- — -
Chemical composition
wt% · log scale- min – max range
- typical value
Mechanical properties
value range by conditionPhysical properties
vs. temperatureChemical composition
| Element | min | max | Similar | Remarks |
|---|---|---|---|---|
| C | 0.01 | |||
| Co | 1 | |||
| Cr | 21 | |||
| Cu | 0.5 | |||
| Fe | 2 | |||
| Mn | 0.8 | |||
| Mo | 17 | |||
| Ni | 61 | Bal | ||
| Si | 0.08 | |||
| W | 1 |
Mechanical properties
| Heat treatment / condition | Yield strength | Tensile strength | Elongation | Reduction of area | Impact energy | Hardness |
|---|---|---|---|---|---|---|
| bars, plates, hot rolled, solution annealed agedhardened | ≥690 | ≥1202 | ≥44.2 | ≥58 | ||
| sheet, cold rolled, solution annealed agedhardened | ≥759 | ≥1230 | ≥40.9 |
Physical properties
20.0
| Elastic modulus | Mean thermal expansion | Thermal conductivity | Specific heat | Resistivity | Density | Poisson's ratio |
|---|---|---|---|---|---|---|
| 223.00 | 11.80 | 412.00 | 0.98 | 8.60;8.64 |