Germany · DIN
TiAl5Sn2.5
DIN 17864:2012 — Titanium and wrought titanium alloys forgings (hammer forgings and drop forgings) - Technical delivery conditions
Chemical composition
wt% · log scale- min – max range
- typical value
Mechanical properties
value range by conditionChemical composition
| Element | min | max | Similar | Remarks |
|---|---|---|---|---|
| Al | 4.5 | 5.5 | ||
| C | 0.08 | |||
| Fe | 0.5 | |||
| H | 0.02 | |||
| N | 0.05 | |||
| O | 0.2 | |||
| Sn | 2 | 3 | ||
| Total Each | 0.1 | |||
| Total Others | 0.4 |
Mechanical properties
| Heat treatment / condition | Yield strength | Tensile strength | Elongation | Reduction of area | Impact energy | Hardness |
|---|---|---|---|---|---|---|
| Drop forging, forgings, 10.00 < t ≤ 100.00mm, annealed | ≤760 | ≤780 | ≤8 | ≤20 |
Physical properties
20.0
| Elastic modulus | Mean thermal expansion | Thermal conductivity | Specific heat | Resistivity | Density | Poisson's ratio |
|---|---|---|---|---|---|---|
| 110.00 | 7.95 | 4.48 |
Typical physical values
| Density | Elastic modulus | Poisson's ratio | Remarks |
|---|---|---|---|
| 4.30–5.10 | 80.00–130.00 | Typical property values for titanium and titanium alloys. These values are not taken from a published standard; they are indicative only and must not be used for design. |
High/low temperature
| Condition | Temperature ℃ | min | max |
|---|---|---|---|
| Drop forging | forgings annealed | 355 | 500 |
| Drop forging | forgings annealed | 380 | 400 |
| Drop forging | forgings annealed | 300 | 455 |
| Drop forging | forgings annealed | 200 | 535 |
Similar grades
| Grade | Region | System |
|---|---|---|
| 3.7115 | DIN |