United States · ASTM

A965 Grade F310

ASTM A965/A965M:2012 — Standard Specification for Steel Forgings,Austenitic,for Pressure and High Temperature Parts(2006a)

Chemical composition

wt% · log scale
0.010.1110100C0.15Cr24 – 26Mn2Ni19 – 22P0.045S0.03Si1
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥205 MPaTensile strength Rm≥515 MPaElongation A≥30 %Reduction of area Z≥35 %

Chemical composition

ElementminmaxSimilarRemarks
C0.15
Cr2426
Mn2
Ni1922
P0.045
S0.03
Si1

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
forgings, Solution annealed≥205≥515≥30 Lo = 50mm≥35