Finland · SFS

X 6 CrNiTi 18 10

SFS EN 10222-5

Chemical composition

wt% · log scale
0.0010.010.1110100C0.08Cr17 – 19Mn2Ni9 – 12P0.045S0.015Si1Ti0.7
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥200 MPaTensile strength Rm510–710 MPaImpact energy Kv/Ku≥60 JElongation A≥30 %Yield strength Rp0.2≥200 MPaTensile strength Rm510–710 MPaImpact energy Kv/Ku≥100 JElongation A≥40 %

High / low temperature

value vs. temperature
80.5180280379479100150200250300350400500°C
  • Condition not stated · Yield strength Rp0.2
  • Condition not stated · Tensile strength Rm

Physical properties

vs. temperature
Elastic modulus GPa
165 – 200°C
Mean thermal expansion 10⁻⁶/K
16.0 – 18.0°C

Creep properties

3.6064.1125185245540550560570580590600610620630640650660670680690700MPa
  • 10000.0h
  • 100000.0h
  • 200000.0h

Temperature °C · time at rupture

Chemical composition

ElementminmaxSimilarRemarks
C0.08
Cr1719
Mn2
Ni912
P0.045
S0.015For products to be machined a controlled sulfur content of 0
Si1
Ti0.7>= 5 x %C

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
forgings, Solution treated, <= 450 mm≥200510–710≥30;≥40≥60 Charpy V Notch; > 10 <= 450 mm;≥100 Charpy V Notch; > 10 <= 450 mm

Physical properties

20.0

Elastic modulusMean thermal expansionThermal conductivitySpecific heatResistivityDensityPoisson's ratio
200.0015.00500.000.737.90

Typical physical values

DensityElastic modulusPoisson's ratioRemarks
7.61–8.10190.00–215.000.27–0.30Typical material properties for stainless steel. These values are not taken from the standard; they are indicative and must not be used for design.
7.86190.00–210.000.27–0.30Material properties for low-carbon, high-alloy steel. These values are not taken from the standard; they are indicative and must not be used for design.

High/low temperature

Yield strength Rp0.2 (MPa)
Temperature ℃Approx.
500119
400125
350130
300136
250147
200157
150167
100176
Tensile strength Rm (MPa)
Temperature ℃Approx.
500360
400375
350375
300375
250385
200390
150410
100440

Fatigue

Test conditions
ItemDetail
ProductSemi Finished products; Thickness: <= 450 mm; Quenched
ExperimentReversed bending; T: 20°C
Specimen
Monotonic
PropertyValue
Yield strength (MPa)190.0
Tensile strength (MPa)500.0 700.0
Elongation (%)30.0
Stress life
No.Cycles
11E7

Creep

Temperature ℃Time hCRS
54010000.0h222.0
540100000.0h154.0
540200000.0h136.0
55010000.0h206.0
550100000.0h142.0
550200000.0h123.0
56010000.0h192.0
560100000.0h129.0
560200000.0h112.0
57010000.0h178.0
570100000.0h118.0
570200000.0h101.0
58010000.0h165.0
580100000.0h107.0
580200000.0h91.0
59010000.0h152.0
590100000.0h96.0
590200000.0h81.0
60010000.0h140.0
600100000.0h86.0
600200000.0h72.0
61010000.0h129.0
610100000.0h77.0
610200000.0h63.0
62010000.0h118.0
620100000.0h68.0
620200000.0h55.0
63010000.0h108.0
630100000.0h60.0
630200000.0h48.0
64010000.0h98.0
640100000.0h53.0
640200000.0h42.0
65010000.0h88.0
650100000.0h46.0
650200000.0h36.0
66010000.0h79.0
660100000.0h40.0
660200000.0h32.0
67010000.0h71.0
670100000.0h35.0
670200000.0h28.0
68010000.0h63.0
680100000.0h31.0
69010000.0h56.0
690100000.0h27.0
70010000.0h49.0

Similar grades

GradeRegionSystem
1.4541ItalyUNI
X 6 CrNiTi 18 10ItalyUNI
1.4541SpainUNE
X 6 CrNiTi 18 10SpainUNE
1.4541RomaniaSTAS
X 6 CrNiTi 18 10RomaniaSTAS
1.4541SwedenSS
X 6 CrNiTi 18 10SwedenSS
1.4541SwitzerlandSNV
X 6 CrNiTi 18 10SwitzerlandSNV
1.4541FinlandSFS
1.4541PolandPN
X 6 CrNiTi 18 10PolandPN
1.4541AustriaONORM
X 6 CrNiTi 18 10AustriaONORM
1.4541NorwayNS
X 6 CrNiTi 18 10NorwayNS
1.4541BelgiumNBN
X 6 CrNiTi 18 10BelgiumNBN
1.4541HungaryMSZ
X 6 CrNiTi 18 10HungaryMSZ
1.4541Czech RepublicCSN
X 6 CrNiTi 18 10Czech RepublicCSN
1.4541BulgariaBDS
X 6 CrNiTi 18 10BulgariaBDS
1.4541United KingdomB.S.
X 6 CrNiTi 18 10United KingdomB.S.
1.4541FranceAFNOR NF
X 6 CrNiTi 18 10FranceAFNOR NF
X 6 CrNiTi 18 10GermanyDIN
1.4541GermanyDIN