International standard · ISO
4007
ISO 6361-2:2011 — ISO 6361-2
Mechanical properties
| Heat treatment / condition | Yield strength | Tensile strength | Elongation | Reduction of area | Impact energy | Hardness |
|---|---|---|---|---|---|---|
| heavy plate, steel strip, Annealed +O, 0.2 < t <= 0.5 mm, sheet | 45 | 110 150.00 | 15 | |||
| heavy plate, steel strip, Annealed +O, 0.5 < t <= 1.5 mm, sheet | 45 | 110 150.00 | 16 | |||
| heavy plate, steel strip, Annealed +O, 1.5 < t <= 3 mm, sheet | 45 | 110 150.00 | 19 | |||
| heavy plate, steel strip, Annealed +O, 3 < t <= 6 mm, sheet | 45 | 110 150.00 | 21 | |||
| heavy plate, steel strip, Annealed +O, 6 < t <= 12.5 mm, sheet | 45 | 110 150.00 | 25 | |||
| heavy plate, steel strip +H111, 0.2 < t <= 0.5 mm, sheet | 45 | 110 150.00 | 15 | |||
| heavy plate, steel strip +H111, 0.5 < t <= 1.5 mm, sheet | 45 | 110 150.00 | 16 | |||
| heavy plate, steel strip +H111, 1.5 < t <= 3 mm, sheet | 45 | 110 150.00 | 19 | |||
| heavy plate, steel strip +H111, 3 < t <= 6 mm, sheet | 45 | 110 150.00 | 21 | |||
| heavy plate, steel strip +H111, 6 < t <= 12.5 mm, sheet | 45 | 110 150.00 | 25 | |||
| heavy plate, steel strip, strain hardened - 1/4 +H12, 0.2 < t <= 0.5 mm, sheet | 110 | 140 180.00 | 4 | |||
| heavy plate, steel strip, strain hardened - 1/4 +H12, 0.5 < t <= 1.5 mm, sheet | 110 | 140 180.00 | 4 | |||
| heavy plate, steel strip, strain hardened - 1/4 +H12, 1.5 < t <= 3 mm, sheet | 110 | 140 180.00 | 5 |