International standard · ISO
7022
ISO 6362-2:2012 — ISO 6362-2
Mechanical properties
value range by conditionMechanical properties
| Heat treatment / condition | Yield strength | Tensile strength | Elongation | Reduction of area | Impact energy | Hardness |
|---|---|---|---|---|---|---|
| Extruded bars, rods, Solution heat treated and artificially aged +T6510, 80 < D or S <= 200 mm | ≤400 | ≤470 | ≤7 | |||
| Extruded bars, rods, Solution heat treated and artificially aged +T6510, D or S <= 80 mm | ≤420 | ≤490 | ≤7 | |||
| Extruded bars, rods, Solution heat treated and artificially aged +T6511, 80 < D or S <= 200 mm | ≤400 | ≤470 | ≤7 | |||
| Extruded bars, rods, Solution heat treated and artificially aged +T6511, D or S <= 80 mm | ≤420 | ≤490 | ≤7 | |||
| Extruded bars, rods, solution heat treated artificially aged, 80 < D or S <= 200 mm | ≤400 | ≤470 | ≤7 | |||
| Extruded bars, rods, solution heat treated artificially aged, D or S <= 80 mm | ≤420 | ≤490 | ≤7 | |||
| Extruded tubes, Solution heat treated and artificially aged +T6510, t <= 30 mm | ≥420 | ≥490 | ≥7 Lo = 5.65√So; A <= 8% in Lo = 50mm | |||
| Extruded tubes, Solution heat treated and artificially aged +T6511, t <= 30 mm | ≥420 | ≥490 | ≥7 Lo = 5.65√So; A <= 8% in Lo = 50mm | |||
| Extruded tubes, solution heat treated artificially aged, t <= 30 mm | ≥420 | ≥490 | ≥7 Lo = 5.65√So; A <= 8% in Lo = 50mm | |||
| extruded profiles, Solution heat treated and artificially aged +T6510, t <= 30 mm | ≥420 | ≥490 | ≥7 Lo = 5.65√So; A <= 8% in Lo = 50mm | |||
| extruded profiles, Solution heat treated and artificially aged +T6511, t <= 30 mm | ≥420 | ≥490 | ≥7 Lo = 5.65√So; A <= 8% in Lo = 50mm | |||
| extruded profiles, solution heat treated artificially aged, t <= 30 mm | ≥420 | ≥490 | ≥7 Lo = 5.65√So; A <= 8% in Lo = 50mm |