Chemical composition

wt% · log scale
0.010.1110C0.22Cr0.3Cr+Ni+Cu0.6Cu0.3Mn1.2 – 1.6Mo0.45 – 0.65Nb0.025 – 0.05Ni0.3P0.035S0.03Si0.15 – 0.5
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥440 MPaTensile strength Rm590–740 MPaElongation A≥17 %Plates, normalized and tempered, 30 < t <=, 60 mmYield strength Rp0.2≥410 MPaTensile strength Rm570–720 MPaElongation A≥17 %Plates, normalized and tempered, 60 < t <=, 100 mmYield strength Rp0.2≥440 MPaTensile strength Rm590–740 MPaImpact energy Kv/Ku≥34 JElongation A≥17 %t 30~60mm, normalized+temperedYield strength Rp0.2≥410 MPaTensile strength Rm570–720 MPaImpact energy Kv/Ku≥34 JElongation A≥17 %t 60~100mm, normalized+tempered

High / low temperature

value vs. temperature
285311338364390200250300350400450°C
  • Plates  Heat treated  60 < t <= 100 mm · Yield strength Rp0.2
  • Plates  Heat treated  30 < t <= 60 mm · Yield strength Rp0.2

Chemical composition

ElementminmaxSimilarRemarks
C0.22
Cr0.3
Cr+Ni+Cu0.6
Cu0.3
Mn1.21.6
Mo0.450.65
Nb0.0250.05
Ni0.3
P0.035
S0.03
Si0.150.5

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
Plates, normalized and tempered, 30 < t <=, 60 mm≥440590–740≥17
Plates, normalized and tempered, 60 < t <=, 100 mm≥410570–720≥17
t 30~60mm, normalized+tempered≥440590–740≥17≥34 Akv transverse
t 60~100mm, normalized+tempered≥410570–720≥17≥34 Akv transverse

High/low temperature

Yield strength Rp0.2 (MPa)
ConditionTemperature ℃Approx.
Plates  Heat treated  60 < t <= 100 mm450295
Plates  Heat treated  60 < t <= 100 mm400315
Plates  Heat treated  60 < t <= 100 mm350330
Plates  Heat treated  60 < t <= 100 mm300340
Plates  Heat treated  60 < t <= 100 mm250350
Plates  Heat treated  60 < t <= 100 mm200360
Plates  Heat treated  30 < t <= 60 mm450315
Plates  Heat treated  30 < t <= 60 mm400335
Plates  Heat treated  30 < t <= 60 mm350350
Plates  Heat treated  30 < t <= 60 mm300360
Plates  Heat treated  30 < t <= 60 mm250370
Plates  Heat treated  30 < t <= 60 mm200380
Impact energy Kv/Ku (J)
ConditionTemperature ℃minRemarks
Plates Heat treated ( transverse )031KV; Average value of 3 test pieces; For transverse direction.