China · GB

40

GB/T 34484.1:2017 — Heat-treatable steels-Part 1:Non-alloy steels

Chemical composition

wt% · log scale
0.010.1110C0.37 – 0.44Cr0.4Cr+Mo+Ni0.63Cu0.3Mn0.5 – 0.8Mo0.1Ni0.4P0.035S0.035Si0.1 – 0.4
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥320 MPaTensile strength Rm≥580 MPaElongation A≥16 %steel products, normalized, <= 20mmYield strength Rp0.2≥260 MPaTensile strength Rm≥530 MPaElongation A≥17 %steel products, normalized, > 100mm <= 310mmYield strength Rp0.2≥290 MPaTensile strength Rm≥550 MPaElongation A≥17 %steel products, normalized, > 20mm <= 100mmYield strength Rp0.2≥400 MPaTensile strength Rm630–780 MPaImpact energy Kv/Ku≥20 JElongation A≥18 %Reduction of area Z≥40 %steel products, quenched and tempered, 20 < d <= 40mm, d

Chemical composition

ElementminmaxSimilarRemarks
C0.370.44
Cr0.4
Cr+Mo+Ni0.63
Cu0.3
Mn0.50.8
Mo0.1
Ni0.4
P0.035
S0.035
Si0.10.4

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
steel products, normalized, <= 20mm≥320≥580≥16
steel products, normalized, > 100mm <= 310mm≥260≥530≥17
steel products, normalized, > 20mm <= 100mm≥290≥550≥17
steel products, quenched and tempered, 20 < d <= 40mm, d≥400630–780≥18≥40≥20
steel products, quenched and tempered, 20 < t <= 60mm, t≥350600–750≥19≥45≥20
steel products, quenched and tempered, 40 < d <= 100mm, d≥350600–750≥19≥45≥20
steel products, quenched and tempered, d <= 20mm, d≥460650–800≥16≥35≥20