Germany · DIN

1.5710

-- — -

Chemical composition

wt% · log scale
0.010.1110C0.32 – 0.4Cr0.3 – 0.7Mn0.4 – 0.8Ni1.25 – 1.75P0.035S0.035Si0.15 – 0.35
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥785 MPaTensile strength Rm980–1180 MPaImpact energy Kv/Ku≥45 JElongation A≥11 %quenched and tempered, <= 16 mmYield strength Rp0.2≥490 MPaTensile strength Rm690–830 MPaImpact energy Kv/Ku≥70 JElongation A≥15 %quenched and tempered, > 100 <= 160 mmYield strength Rp0.2≥685 MPaTensile strength Rm880–1030 MPaImpact energy Kv/Ku≥55 JElongation A≥13 %quenched and tempered, > 16 <= 40 mmYield strength Rp0.2≥590 MPaTensile strength Rm780–930 MPaImpact energy Kv/Ku≥65 JElongation A≥14 %quenched and tempered, > 40 <= 100 mm

Chemical composition

ElementminmaxSimilarRemarks
C0.320.4
Cr0.30.7
Mn0.40.8
Ni1.251.75
P0.035
S0.035
Si0.150.35

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
quenched and tempered, <= 16 mm≥785980–1180≥11≥45 ISO-V (DVM)
quenched and tempered, > 100 <= 160 mm≥490690–830≥15≥70 ISO-V (DVM)
quenched and tempered, > 16 <= 40 mm≥685880–1030≥13≥55 ISO-V (DVM)
quenched and tempered, > 40 <= 100 mm≥590780–930≥14≥65 ISO-V (DVM)

Heat treatment

Type1
Heat-treatment curve淬透性
Heat-treatment curveTempered