Germany · DIN
1.2313
-- — -
Chemical composition
wt% · log scale- min – max range
- typical value
Mechanical properties
value range by conditionHigh / low temperature
value vs. temperature- Condition not stated · Tensile strength Rm
Chemical composition
| Element | min | max | Similar | Remarks |
|---|---|---|---|---|
| C | 0.16 | 0.23 | ||
| Cr | 2.3 | 2.6 | ||
| Mn | 0.2 | 0.4 | ||
| Mo | 0.3 | 0.4 | ||
| P | 0.025 | |||
| S | 0.025 | |||
| Si | 0.2 | 0.4 |
Mechanical properties
| Heat treatment / condition | Yield strength | Tensile strength | Elongation | Reduction of area | Impact energy | Hardness |
|---|---|---|---|---|---|---|
| soft annealed | HB ≤200 HB30 |
High/low temperature
| Temperature ℃ | Approx. |
|---|---|
| 700 | 880 |
| 650 | 980 |
| 600 | 1080 |
| 550 | 1180 |
| 500 | 1270 |
| 450 | 1370 |
| 400 | 1420 |