Germany · DIN

StE 355

DIN 17102:1983 — DIN 17102

Chemical composition

ElementminmaxSimilarRemarks
Al0.02If nitrogen is additionally fixed by niobiumIf nitrogen is additionally fixed by niobium
C0.2
Cr0.3
Cr+Cu+Mo0.45
Cu0.2
Mn0.91.65
Mo0.08
Nb0.05
Nb+Ti+V0.12
Ni0.3If Ni is added as an alloying elementIf Ni is added as an alloying element
P0.035
S0.03
Si0.10.5
V0.1

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
bars, sections 100 < t ≤ 125mm, hot rolled, flats305460 600.0022
bars, sections 125 < t ≤ 150mm, hot rolled, flats295450 590.0022
bars, sections 35 < t ≤ 50mm, hot rolled, flats345490 630.0022
bars, sections 50 < t ≤ 70mm, hot rolled, flats335490 630.0022
bars, sections 70 < t ≤ 85mm, hot rolled, flats325480 620.0022
bars, sections 85 < t ≤ 100mm, hot rolled, flats315470 610.0022
bars, sections t ≤ 35mm, hot rolled, flats355490 630.0022

Physical properties

-100.0

Elastic modulusMean thermal expansionThermal conductivitySpecific heatResistivityDensityPoisson's ratio
217.0010.8037.60371.000.18

Typical physical values

DensityElastic modulusPoisson's ratioRemarks
7.86203.000.27–0.30低碳,低合金钢的典型性能数值。此值不来源于标准,它是指示性指标,不能被用于设计用途。

Similar grades

GradeRegionSystem
StE 355GermanySEW
1.0562GermanyDIN