European Union · EN
DC 06 + ZE
EN 10152:2009 — EN 10152
Chemical composition
wt% · log scale- min – max range
- typical value
Mechanical properties
value range by conditionChemical composition
| Element | min | max | Similar | Remarks |
|---|---|---|---|---|
| C | 0.02 | |||
| Mn | 0.25 | |||
| P | 0.02 | |||
| S | 0.02 | |||
| Ti | 0.3 | Titanium may be replaced by NB. C and N shall be completely bound. |
Mechanical properties
| Heat treatment / condition | Yield strength | Tensile strength | Elongation | Reduction of area | Impact energy | Hardness |
|---|---|---|---|---|---|---|
| cold rolledheavy plate, skin passed, 0.35 < t <= 0.5 mm | 130–220 | 270–350 | ≥37 Lo = 80 mm | |||
| cold rolledheavy plate, skin passed, 0.50 < t <= 0.70 mm | 130–200 | 270–350 | ≥39 Lo = 80 mm | |||
| cold rolledheavy plate, skin passed, 0.70 < t <= 3 mm | 130–190 | 270–350 | ≥37 Lo = 80 mm |