France · AFNOR NF
51 CrV 4
NF EN 10250-3
Chemical composition
| Element | min | max | Similar | Remarks |
|---|---|---|---|---|
| C | 0.47 | 0.55 | ||
| Cr | 0.9 | 1.2 | ||
| Mn | 0.7 | 1.1 | ||
| P | 0.035 | |||
| S | 0.035 | |||
| Si | 0.4 | |||
| V | 0.1 | 0.25 |
Mechanical properties
| Heat treatment / condition | Yield strength | Tensile strength | Elongation | Reduction of area | Impact energy | Hardness |
|---|---|---|---|---|---|---|
| die forgings, forgings, quenched and tempered, <= 160 mm, forged bars | 600 | 800 | 9;13 | 16;30 |
Physical properties
| Elastic modulus | Mean thermal expansion | Thermal conductivity | Specific heat | Resistivity | Density | Poisson's ratio |
|---|---|---|---|---|---|---|
| 210.00 |
Typical physical values
| Density | Elastic modulus | Poisson's ratio | Remarks |
|---|---|---|---|
| 7.72–8.00 | 190.00–210.00 | 0.27–0.30 | 典型属性数值,工具钢。此值不来源于标准,它是指示性指标,不能被用于设计用途。 |
| 7.85 | 200.00–207.00 | 0.27–0.30 | 低碳钢低合金钢的材料性能属性数值,此值不来源于标准,它是指示性指标,不能被用于设计用途。 |
Heat treatment
| Type | 1 |
|---|---|
| Heat-treatment curve | CCT modified |
| Heat-treatment curve | Hardness-Tempering |
| Heat-treatment curve | CCT |
| Heat-treatment curve | TTT |
| Heat-treatment curve | 淬透性 |
Similar grades
| Grade | Region | System |
|---|---|---|
| 1.8159 | UNI | |
| 51 CrV 4 | UNI | |
| 1.8159 | UNE | |
| 1.8159 | STAS | |
| 51 CrV 4 | STAS | |
| 1.8159 | SS | |
| 51 CrV 4 | SS | |
| 1.8159 | SNV | |
| 51 CrV 4 | SNV | |
| 1.8159 | SFS | |
| 51 CrV 4 | SFS | |
| 1.8159 | PN | |
| 51 CrV 4 | PN | |
| 1.8159 | ONORM | |
| 51 CrV 4 | ONORM | |
| 1.8159 | NS | |
| 1.8159 | NBN | |
| 1.8159 | MSZ | |
| 51 CrV 4 | DIN | |
| 1.8159 | Czech Republic | CSN |
| 51 CrV 4 | Czech Republic | CSN |
| 1.8159 | Bulgaria | BDS |
| 51 CrV 4 | Bulgaria | BDS |
| 1.8159 | B.S. | |
| 1.8159 | AFNOR NF | |
| 51 CrV 4 | MSZ | |
| 51 CrV 4 | NS | |
| 51 CrV 4 | NBN | |
| 51 CrV 4 | UNE | |
| GS-50 CrV 4 | SEW | |
| 50 CrV 4 | DIN | |
| 1.8159 | DIN | |
| 51 CrV 4 | B.S. |