Chemical composition

wt% · log scale
0.010.11C0.07 – 0.14Cr0.15Cu0.3Mn0.25 – 0.5Ni0.3P0.035S0.04Si0.07
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥196 MPaTensile strength Rm≥314 MPaElongation A≥25 %steel tubes, Heat treatedYield strength Rp0.2≥176 MPaTensile strength Rm≥372 MPasteel tubes, not heat treated, t= 10 - 19 mmYield strength Rp0.2≥176 MPaTensile strength Rm≥333 MPasteel tubes, not heat treated, t= 19 - 60 mmYield strength Rp0.2≥176 MPaTensile strength Rm≥314 MPasteel tubes, not heat treated, t= 60 - 152 mm

Physical properties

vs. temperature
Mean thermal expansion 10⁻⁶/K
12.4 – 15.3°C
Thermal conductivity W/(m·K)
27.0 – 58.0°C
Specific heat J/(kg·K)
466 – 567°C

Chemical composition

ElementminmaxSimilarRemarks
C0.070.14
Cr0.15
Cu0.3
Mn0.250.5
Ni0.3
P0.035
S0.04
Si0.07

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
steel tubes, Heat treated≥196≥314≥25
steel tubes, not heat treated, t= 10 - 19 mm≥176≥372
steel tubes, not heat treated, t= 19 - 60 mm≥176≥333
steel tubes, not heat treated, t= 60 - 152 mm≥176≥314

Physical properties

20.0

Elastic modulusMean thermal expansionThermal conductivitySpecific heatResistivityDensityPoisson's ratio
186.007.86

Typical physical values

DensityElastic modulusPoisson's ratioRemarks
7.86203.000.27–0.30低碳,低合金钢的典型性能数值。此值不来源于标准,它是指示性指标,不能被用于设计用途。

Similar grades

GradeRegionSystem
1008United StatesSAE
1.0038GermanyDIN