Romania · STAS

1.8901

SR EN 10025-3

Chemical composition

wt% · log scale
0.0010.010.1110Al0.015C0.22CEV0.53Cr0.35Cr+Mo0.38Cu0.6Mn0.95 – 1.8Mo0.13N0.027Nb0.06Ni0.85P0.035S0.03Si0.65Ti0.06V0.22V+Nb+Ti0.26
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥380 MPaTensile strength Rm530–710 MPaElongation A≥17 %hot rolled , normalized, 100.0 < t <= 150.0 mmYield strength Rp0.2≥370 MPaTensile strength Rm530–710 MPaElongation A≥17 %hot rolled , normalized, 150.0 < t <= 200.0 mmYield strength Rp0.2≥440 MPaTensile strength Rm540–720 MPaElongation A≥17 %hot rolled , normalized, 16.0 < t <= 40.0 mmYield strength Rp0.2≥430 MPaTensile strength Rm540–720 MPaElongation A≥17 %hot rolled , normalized, 40.0 < t <= 63.0 mm

High / low temperature

value vs. temperature
17.224.431.538.645.8-20-10°C
  • hot-rolled products normalized ( transverse ) · Impact energy Kv/Ku
  • hot-rolled products normalized ( longitudinal ) · Impact energy Kv/Ku

Chemical composition

ElementminmaxSimilarRemarks
Al0.015If sufficient nitrogen-binding elemets are present
C0.22
CEV0.53for t <= 63mm; CEV = max.0.54 for 63 < t <= 100mm; CEV = max.0.55 for 100 < t <= 250mm
Cr0.35
Cr+Mo0.38
Cu0.6Cu content above 0
Mn0.951.8
Mo0.13
N0.027
Nb0.06
Ni0.85
P0.035For long products the P content can be 0
S0.03For long products the S content can be 0
Si0.65
Ti0.06
V0.22
V+Nb+Ti0.26

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
hot rolled , normalized, 100.0 < t <= 150.0 mm≥380530–710≥17 Lo=5.65√So
hot rolled , normalized, 150.0 < t <= 200.0 mm≥370530–710≥17 Lo=5.65√So
hot rolled , normalized, 16.0 < t <= 40.0 mm≥440540–720≥17 Lo=5.65√So
hot rolled , normalized, 40.0 < t <= 63.0 mm≥430540–720≥17 Lo=5.65√So
hot rolled , normalized, 63.0 < t <= 80.0 mm≥410540–720≥17 Lo=5.65√So
hot rolled , normalized, 80.0 < t <= 100.0 mm≥400540–720≥17 Lo=5.65√So
hot rolled , normalized, t <= 16.0 mm≥460540–720≥17 Lo=5.65√So
hot rolled , normalized≥20 Charpy V Notch (-20°C);≥24 Charpy V Notch (-10°C);≥27 Charpy V Notch (0°C);≥31 Charpy V Notch (20°C);≥40 Charpy V Notch (-20°C); Corresponds with 27J at -30°C;≥43 Charpy V Notch (-10°C);≥47 Charpy V Notch (0°C);≥55 Charpy V Notch (20°C)

High/low temperature

Impact energy Kv/Ku (J)
ConditionTemperature ℃minRemarks
hot-rolled products normalized ( transverse )-1024Charpy V Notch
hot-rolled products normalized ( transverse )-2020Charpy V Notch
hot-rolled products normalized ( longitudinal )-1043Charpy V Notch
hot-rolled products normalized ( longitudinal )-2040Charpy V Notch; Coresponds to 27J at (-30°C)