Italy · UNI
C 40 R
UNI EN 10083-1 — Steels for quenching and tempering - Part 1 : general technical delivery conditions
Chemical composition
wt% · log scale- min – max range
- typical value
Mechanical properties
value range by conditionChemical composition
| Element | min | max | Similar | Remarks |
|---|---|---|---|---|
| C | 0.37 | 0.44 | ||
| Cr | 0.4 | |||
| Cr+Mo+Ni | 0.63 | If steels are ordered without mechanical requirements in the quenched and tempered or normalized condition | ||
| Mn | 0.5 | 0.8 | ||
| Mo | 0.1 | |||
| Ni | 0.4 | |||
| P | 0.035 | |||
| S | 0.02 | 0.04 | Steels with improved machinability as a result of the addition of lead or higher sulphur contents up to around 0 | |
| Si | 0.4 |
Mechanical properties
| Heat treatment / condition | Yield strength | Tensile strength | Elongation | Reduction of area | Impact energy | Hardness |
|---|---|---|---|---|---|---|
| bars, open die forgings and die forgings +N, 100 mm < d <= 250 mm, flats | 260.00 | 530.00 | 17.00 | |||
| bars, open die forgings and die forgings +N, 16 mm < d <= 100 mm, flats | 290.00 | 550.00 | 17.00 | |||
| bars, open die forgings and die forgings +N, d <= 16 mm or t <= 16 mm, flats | 320.00 | 580.00 | 16.00 | |||
| bars, open die forgings and die forgings +QT, 16 < d +MM < 40 or 8 < t +MM <= 20 | T - thickness) | T - thickness) | T - thickness) | T - thickness) | T - thickness) | |
| bars, open die forgings and die forgings +QT, 40 < d +MM < 100 or 20 < t +MM <= 60 | T - thickness) | T - thickness) | T - thickness) | T - thickness) | T - thickness) | |
| bars, open die forgings and die forgings +QT, d <= 16 mm or t <= 8 mm | T - thickness) | T - thickness) | T - thickness) | T - thickness) | T - thickness) |
Heat treatment
| Type | 1 |
|---|---|
| Heat-treatment curve | Hardness-Tempering |
| Heat-treatment curve | CCT |
| Heat-treatment curve | Hardenability |