Spain · UNE

1.4477

UNE EN 10088-3

Chemical composition

wt% · log scale
0.0010.010.1110100C0.03Cr28 – 30Cu0.8Mn0.8 – 1.5Mo1.5 – 2.6N0.3 – 0.4Ni5.8 – 7.5P0.03S0.015Si0.5
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥650 MPaTensile strength Rm800–1050 MPaImpact energy Kv/Ku≥100 JElongation A≥25 %HardnessHBrods, bars, wire, sections, bright products +AT, <= 10 mmYield strength Rp0.2≥550 MPaTensile strength Rm750–1000 MPaImpact energy Kv/Ku≥100 JElongation A≥25 %HardnessHBrods, bars, wire, sections, bright products +AT, > 10 <= 160 mm

High / low temperature

value vs. temperature
382429475522568100150200250°C
  • solution annealed +AT 10 < t <= 160mm +T · Yield strength Rp0.2
  • solution annealed +AT t <= 10mm +T · Yield strength Rp0.2

Physical properties

vs. temperature
Elastic modulus GPa
180 – 200°C
Mean thermal expansion 10⁻⁶/K
11.5 – 12.5°C

Chemical composition

ElementminmaxSimilarRemarks
C0.03
Cr2830
Cu0.8
Mn0.81.5
Mo1.52.6
N0.30.4
Ni5.87.5
P0.03
S0.015
Si0.5

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
rods, bars, wire, sections, bright products +AT, <= 10 mm≥650800–1050≥25 After fracture; (trans.)≥100 KV (ISO-V) (trans.)HB ≤310
rods, bars, wire, sections, bright products +AT, > 10 <= 160 mm≥550750–1000≥25 After fracture; (trans.)≥100 KV (ISO-V) (trans.)HB ≤310

Physical properties

20.0

Elastic modulusMean thermal expansionThermal conductivitySpecific heatResistivityDensityPoisson's ratio
200.0013.00470.000.807.70

Typical physical values

DensityElastic modulusPoisson's ratioRemarks
7.61–8.10190.00–215.000.27–0.30Typical material properties for stainless steel. These values are not taken from the standard; they are indicative and must not be used for design.
7.86190.00–210.000.27–0.30Material properties for low-carbon, high-alloy steel. These values are not taken from the standard; they are indicative and must not be used for design.

High/low temperature

Yield strength Rp0.2 (MPa)
ConditionTemperature ℃Approx.
solution annealed +AT 10 < t <= 160mm +T250400
solution annealed +AT 10 < t <= 160mm +T200430
solution annealed +AT 10 < t <= 160mm +T150460
solution annealed +AT 10 < t <= 160mm +T100500
solution annealed +AT t <= 10mm +T250440
solution annealed +AT t <= 10mm +T200470
solution annealed +AT t <= 10mm +T150500
solution annealed +AT t <= 10mm +T100550

Similar grades

GradeRegionSystem
1.4477ItalyUNI
X2CrNiMoN29-7-2ItalyUNI
X2CrNiMoN29-7-2SpainUNE
1.4477RomaniaSTAS
X2CrNiMoN29-7-2RomaniaSTAS
1.4477SwedenSS
X2CrNiMoN29-7-2SwedenSS
1.4477SwitzerlandSNV
X2CrNiMoN29-7-2SwitzerlandSNV
1.4477FinlandSFS
X2CrNiMoN29-7-2FinlandSFS
1.4477PolandPN
X2CrNiMoN29-7-2PolandPN
1.4477AustriaONORM
X2CrNiMoN29-7-2AustriaONORM
1.4477NorwayNS
X2CrNiMoN29-7-2NorwayNS
1.4477BelgiumNBN
X2CrNiMoN29-7-2BelgiumNBN
1.4477HungaryMSZ
X2CrNiMoN29-7-2HungaryMSZ
1.4477GermanyDIN
X2CrNiMoN29-7-2GermanyDIN
1.4477Czech RepublicCSN
X2CrNiMoN29-7-2Czech RepublicCSN
1.4477BulgariaBDS
X2CrNiMoN29-7-2BulgariaBDS
1.4477United KingdomB.S.
X2CrNiMoN29-7-2United KingdomB.S.
1.4477FranceAFNOR NF
X2CrNiMoN29-7-2FranceAFNOR NF