Hungary · MSZ

1.0382

MSZ EN 10202

Chemical composition

wt% · log scale
0.0010.010.11Al0.02 – 0.08As0.02C0.04 – 0.08Cr0.08Cu0.08Mn0.18 – 0.35Mo0.02N0.008Other0.02P0.02S0.02Si0.03Sn0.02
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≤580 MPaTensile strength Rm≤590 MPa

Chemical composition

ElementminmaxSimilarRemarks
Al0.020.08
As0.02
C0.040.08For Type B: %C=0.09-0.12
Cr0.08
Cu0.08
Mn0.180.35For Type B: %Mn=0.30-0.50
Mo0.02
N0.008
Other0.02
P0.02
S0.02
Si0.03
Sn0.02

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
coil, heavy plate, x <= 0.21 mm, x -≤580≤590