Sweden · SS

L 360 NB

SS EN 10208-2

Chemical composition

wt% · log scale
0.0010.010.1110Al0.015 – 0.06C0.2CEV0.45Cr0.3Cu0.25Mn1.6Mo0.1N0.012Nb0.05Ni0.3P0.025S0.02Si0.45Ti0.04V0.1V+Nb+Ti0.15
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2360–510 MPaTensile strength Rm≥460 MPaElongation A≥20 %

Chemical composition

ElementminmaxSimilarRemarks
Al0.0150.06Al/N >= 2:1
C0.2
CEV0.45CEV= C + Mn/6 + (Cr+Mo+V)/5 + (Cr+Ni)/15; the CEV is only specified for the product analysis.For grades with values higher than 0
Cr0.3
Cu0.25
Mn1.6For each reduction of 0
Mo0.1
N0.012
Nb0.05
Ni0.3
OtherChemical composition for larger wall thicknesses up to 40 mm is to be agreed.
P0.025
S0.02
Si0.45
Ti0.04
V0.1
V+Nb+Ti0.15

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
steel tubes +N, <= 25 mm360–510 Yield stress is Rt0≥460≥20 For transverse specimens; for longitudinal specimens the values of A shall be 2 units higher.