Chemical composition

wt% · log scale
0.0010.010.1110Al0.02C0.15Cr0.3Cu0.3Mn0.4 – 1.2Mo0.08Nb0.01Ni0.3P0.025S0.02Si0.35Ti0.03V0.02
  • min – max range
  • typical value

Mechanical properties

value range by condition
Impact energy Kv/Ku≥55 JImpact energy Kv/Ku≥45 JImpact energy Kv/Ku≥40 Jwelded steel tube, <= 10 mmYield strength Rp0.2≥215 MPaTensile strength Rm360–480 MPaElongation A≥25 %welded steel tube +N, <= 10 mm

High / low temperature

value vs. temperature
39.441.042.544.045.6-40-20°C
  • welded steel tubes <= 10 mm (t) · Impact energy Kv/Ku

Chemical composition

ElementminmaxSimilarRemarks
Al0.02Al/N=>2
C0.15
Cr0.3
Cu0.3
Mn0.41.2
Mo0.08
Nb0.01
Ni0.3
P0.025
S0.02
Si0.35
Ti0.03
V0.02

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
welded steel tube, <= 10 mm≥55 Charpy V Notch (20°C);≥45 Charpy V Notch (-20°C);≥40 Charpy V Notch (-40°C)
welded steel tube +N, <= 10 mm≥215360–480≥25 long. test

High/low temperature

Impact energy Kv/Ku (J)
ConditionTemperature ℃minRemarks
welded steel tubes <= 10 mm (t)-2045Charpy V Notch
welded steel tubes <= 10 mm (t)-4040Charpy V Notch