Finland · SFS

12NiCr3-2

SFS EN 10263-3

Chemical composition

wt% · log scale
0.010.1110C0.09 – 0.15Cr0.4 – 0.7Cu0.25Mn0.3 – 0.6Ni0.5 – 0.8P0.025S0.025Si0.3
  • min – max range
  • typical value

Mechanical properties

value range by condition
Tensile strength Rm500.00Reduction of area Z64 %bars, wire +U+C+AC, > 2 <= 5 mm, steel barsTensile strength Rm480.00Reduction of area Z64 %bars, wire +U+C+AC, > 5 <= 40 mm, steel barsTensile strength Rm540.00Reduction of area Z62 %bars, wire +U+C+AC+LC, > 2 <= 5 mm, steel barsTensile strength Rm520.00Reduction of area Z62 %bars, wire +U+C+AC+LC, > 5 <= 40 mm, steel bars

Chemical composition

ElementminmaxSimilarRemarks
C0.090.15
Cr0.40.7
Cu0.25
Mn0.30.6
Ni0.50.8
P0.025
S0.025
Si0.3A lower silicon content or a specific silicon range may be agreed at the time of ordering.

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
bars, wire +U+C+AC, > 2 <= 5 mm, steel bars500.0064
bars, wire +U+C+AC, > 5 <= 40 mm, steel bars480.0064
bars, wire +U+C+AC+LC, > 2 <= 5 mm, steel bars540.0062
bars, wire +U+C+AC+LC, > 5 <= 40 mm, steel bars520.0062
bars, wire +AC, > 5 <= 40 mm, steel bars500.0062
bars, wire +AC+C, > 10 <= 40 mm, steel bars610.0059
bars, wire +AC+C, > 5 <= 10 mm, steel bars620.0059
bars, wire, -+FP, > 5 <= 40 mm, HBSteel bar 130 180.00

Heat treatment

Type1
Heat-treatment curveHardness-Tempering
Heat-treatment curveCCT modified
Heat-treatment curveHardenability