Global · Enterprise standard
NILO 42
-- — -
Mechanical properties
value range by conditionHigh / low temperature
value vs. temperature- hot rolled bars annealed · Yield strength Rp0.2
- hot rolled bars annealed · Tensile strength Rm
Physical properties
vs. temperatureChemical composition
| Element | min | max | Similar | Remarks |
|---|---|---|---|---|
| Fe | 58 | |||
| Ni | 42 |
Mechanical properties
| Heat treatment / condition | Yield strength | Tensile strength | Elongation | Reduction of area | Impact energy | Hardness |
|---|---|---|---|---|---|---|
| hot rolledbars, annealed | ≥250 | ≥490 | ≥43 Lo= 50 mm |
Physical properties
20.0
| Elastic modulus | Mean thermal expansion | Thermal conductivity | Specific heat | Resistivity | Density | Poisson's ratio |
|---|---|---|---|---|---|---|
| 10.50 | 0.61 | 8.11 |
Typical physical values
| Density | Elastic modulus | Poisson's ratio | Remarks |
|---|---|---|---|
| 7.90–8.80 | 185.00–205.00 | 0.32–0.34 | 镍合金:incoalloy |
| 7.80 | 190.00–210.00 | 0.27–0.30 | 电工钢材料性能属性数值,此值不来源于标准,它是指示性指标,不能被用于设计用途。 |
| 7.86 | 190.00–210.00 | 0.27–0.30 | 低碳,高合金钢材料性能属性数值,此值不来源于标准,它是指示性指标,不能被用于设计用途。 |
High/low temperature
| Condition | Temperature ℃ | Approx. |
|---|---|---|
| hot rolled bars annealed | 600 | 93 |
| hot rolled bars annealed | 500 | 93 |
| hot rolled bars annealed | 400 | 93 |
| hot rolled bars annealed | 300 | 110 |
| hot rolled bars annealed | 200 | 130 |
| hot rolled bars annealed | 100 | 210 |
| Condition | Temperature ℃ | Approx. |
|---|---|---|
| hot rolled bars annealed | 600 | 210 |
| hot rolled bars annealed | 500 | 310 |
| hot rolled bars annealed | 400 | 370 |
| hot rolled bars annealed | 300 | 410 |
| hot rolled bars annealed | 200 | 450 |
| hot rolled bars annealed | 100 | 450 |