Global · Enterprise standard
INCOLOY MA956
-- — -
Chemical composition
wt% · log scale- min – max range
- typical value
Mechanical properties
value range by conditionPhysical properties
vs. temperatureChemical composition
| Element | min | max | Similar | Remarks |
|---|---|---|---|---|
| Al | 3.75 | 5.75 | ||
| C | 0.1 | |||
| Co | 0.3 | |||
| Cr | 18.5 | 21.5 | ||
| Cu | 0.15 | |||
| Mn | 0.3 | |||
| Ni | 0.5 | |||
| P | 0.02 | |||
| Si | 0.05 | |||
| Ti | 0.2 | 0.6 | ||
| Y2O3 | 0.3 | 0.7 |
Mechanical properties
| Heat treatment / condition | Yield strength | Tensile strength | Elongation | Reduction of area | Impact energy | Hardness |
|---|---|---|---|---|---|---|
| Cold rolled sheets, annealed | ≥545 | ≥650 |
Physical properties
20.0
| Elastic modulus | Mean thermal expansion | Thermal conductivity | Specific heat | Resistivity | Density | Poisson's ratio |
|---|---|---|---|---|---|---|
| 10.90 | 469.00 | 1.31 | 7.25 |
Typical physical values
| Density | Elastic modulus | Poisson's ratio | Remarks |
|---|---|---|---|
| 7.61–8.10 | 190.00–215.00 | 0.27–0.30 | Typical material properties for stainless steel. These values are not taken from the standard; they are indicative and must not be used for design. |
| 7.86 | 190.00–210.00 | 0.27–0.30 | Material properties for low-carbon, high-alloy steel. These values are not taken from the standard; they are indicative and must not be used for design. |