Sweden · SS

DC 07

SS EN 10130:2006 — SS EN 10130

Chemical composition

wt% · log scale
0.0010.010.11C0.01Mn0.2P0.02S0.02Ti0.2
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2100–130 MPaTensile strength Rm250–310 MPaElongation A≥42 %cold rolledheavy plate, skin passed, 0.5 < t <= 0.7 mmYield strength Rp0.2100–110 MPaTensile strength Rm250–310 MPaElongation A≥40 %cold rolledheavy plate, skin passed, t <= 0.5 mmYield strength Rp0.2100–150 MPaTensile strength Rm250–310 MPaElongation A≥40 %cold rolledheavy plate, skin passed, t > 0.7 mm

Chemical composition

ElementminmaxSimilarRemarks
C0.01
Mn0.2
P0.02
S0.02
Ti0.2May be replaced by Nb. Carbon and nitrogen shall be completely bound.

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
cold rolledheavy plate, skin passed, 0.5 < t <= 0.7 mm100–130250–310≥42 Lo = 80 mm
cold rolledheavy plate, skin passed, t <= 0.5 mm100–110250–310≥40 Lo = 80 mm
cold rolledheavy plate, skin passed, t > 0.7 mm100–150250–310≥40 Lo = 80 mm