Chemical composition

wt% · log scale
0.010.1110C0.03 – 0.1Cr0.2Cu0.3Mn1.4Mo0.3 – 0.6Nb0.05Ni0.6 – 1.2P0.02S0.02Si0.9V0.05
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥890 MPaTensile strength Rm940–1180 MPaImpact energy Kv/Ku≥47 JElongation A≥15 %

Chemical composition

ElementminmaxSimilarRemarks
C0.030.1
Cr0.2
Cu0.3
Mn1.4
Mo0.30.6
Nb0.05
Ni0.61.2
P0.02
S0.02
Si0.9
V0.05

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
electrodes≥890940–1180≥15≥47 Charpy V Notch (-30°C)

High/low temperature

Impact energy Kv/Ku (J)
ConditionTemperature ℃minRemarks
electrodes-3047Charpy V Notch