Australia · AS
S - Ni Cr 20 3
AS 1833:2002 — Austenitic Cast Iron
Chemical composition
wt% · log scale- min – max range
- typical value
Mechanical properties
value range by conditionChemical composition
| Element | min | max | Similar | Remarks |
|---|---|---|---|---|
| C | 3 | |||
| Cr | 2.5 | 3.5 | ||
| Cu | 0.5 | |||
| Mn | 0.5 | 1.5 | ||
| Ni | 18 | 22 | ||
| P | 0.08 | |||
| Si | 1.5 | 3 |
Mechanical properties
| Heat treatment / condition | Yield strength | Tensile strength | Elongation | Reduction of area | Impact energy | Hardness |
|---|---|---|---|---|---|---|
| castings, cast or heat treated | 210–260 | 390–490 | 7–15 | ≥12 Charpy V-Notch | HB 150–255 |
Physical properties
20.0
| Elastic modulus | Mean thermal expansion | Thermal conductivity | Specific heat | Resistivity | Density | Poisson's ratio |
|---|---|---|---|---|---|---|
| 7.40 |
Similar grades
| Grade | Region | System |
|---|---|---|
| S - Ni Cr 20 3 | International standard | ISO |
| ASG Ni20Cr3 | IS | |
| FCDA-NiCr 20 3 | JIS | |
| S-Ni Cr 20 3 | UNI |