China · Wugang Q/WTB

WDB620E

WJX 044:2011 — WJX 044

Chemical composition

wt% · log scale
0.0010.010.1110B0.003C0.07Cr0.3Cu0.3Mn1 – 1.6Mo0.3Nb0.08Ni0.3P0.02S0.01Si0.15 – 0.4V0.08
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥490 MPaTensile strength Rm620–750 MPaElongation A≥17 %

Chemical composition

ElementminmaxSimilarRemarks
B0.003
C0.07
Cr0.3
Cu0.3
Mn11.6
Mo0.3
Nb0.08
Ni0.3
P0.02
S0.01
Si0.150.4
V0.08

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
steel plates, TMCP+tempered, 8 <= t <= 30mm, t≥490620–750≥17

High/low temperature

Impact energy Kv/Ku (J)
ConditionTemperature ℃min
steel plates TMCP+ tempered 8 <= t <= 30mm t-4034