International standard · ISO

4876-088-00-I

ISO 15510:2010 — Stainless steels. Chemical composition

Chemical composition

wt% · log scale
0.0010.010.1110100Al0.15 – 0.6C0.1Cr19 – 23Cu0.7Mn1.5Ni30 – 34P0.015S0.015Si1Ti0.15 – 0.6
  • min – max range
  • typical value

Physical properties

vs. temperature
Elastic modulus GPa
125 – 200°C
Mean thermal expansion 10⁻⁶/K
15.0 – 19.0°C
Thermal conductivity W/(m·K)
12.0 – 17.0°C
Specific heat J/(kg·K)
460 – 550°C
Resistivity Ω·mm²/m
0.990 – 1.00°C
Density kg/dm³
8.00 – 8.00°C

Creep properties

-19.641.2102163224600700710720730740750760770780790800810820830840850860870880890900910920930940950MPa
  • 1000.0h
  • 10000.0h
  • 30000.0h
  • 100000.0h
  • 200000.0h

Temperature °C · time at rupture

Chemical composition

ElementminmaxSimilarRemarks
Al0.150.6
C0.1
Cr1923
Cu0.7
Mn1.5
Ni3034
P0.015
S0.015
Si1
Ti0.150.6

Physical properties

20.0

Elastic modulusMean thermal expansionThermal conductivitySpecific heatResistivityDensityPoisson's ratio
200.0012.00460.00;550.000.99;1.008.00

Creep

1. Solution-annealed (+AT) Bars, flat products, forgings, sections, rods, wires

Temperature ℃Time hRp1CRS
6001000.0h130.0200.0
60010000.0h90.0152.0
7001000.0h70.090.0
70010000.0h40.068.0
8001000.0h30.045.0
80010000.0h15.030.0
9001000.0h13.020.0
90010000.0h5.010.0

Similar grades

GradeRegionSystem
1.4959European UnionEN
1.4876European UnionEN
X 8 NiCrAlTi 32 21European UnionEN
X 10 NiCrAlTi 32 21European UnionEN
X 5 NiCrAlTi 31 20GermanyDIN
1.4958GermanyDIN