China · GB

RuTSi4Mo

GB/T 26653:2011 — Exhaust manifold iron castings

Chemical composition

wt% · log scale
0.010.1110C2.8 – 3.6Cr0.5Cu0.5Mn0.3Mo0.5 – 0.7Ni0.6P0.05S0.02Si4.3 – 4.7Ti0.2
  • min – max range
  • typical value

Mechanical properties

value range by condition
Yield strength Rp0.2≥400 MPaTensile strength Rm≥480 MPaElongation A≥2 %HardnessHB

Chemical composition

ElementminmaxSimilarRemarks
C2.83.6
Cr0.5
Cu0.5
Mn0.3
Mo0.50.7
Ni0.6
P0.05
S0.02
Si4.34.7
Ti0.2

Mechanical properties

Heat treatment / conditionYield strengthTensile strengthElongationReduction of areaImpact energyHardness
castings≥400≥480≥2HB 200–260 HBW